Physical Properties | Metric | English | Comments |
---|
Bulk Density | 0.730 g/cc | 0.0264 lb/in³ |
Density | >= 1.27 g/cc | >= 0.0459 lb/in³ |
Water Absorption | <= 0.15 % | <= 0.15 % |
Viscosity Test | 76 - 80 cm³/g | 0.76 - 0.80 dl/g |
ASTM Color | <= 1.0 | <= 1.0 |
| >= 64 | >= 64 |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength | 50.0 MPa | 7250 psi |
Tensile Strength, Yield | 50.0 MPa | 7250 psi |
Elongation at Break | 84 % | 84 % |
Elongation at Yield | 4.2 % | 4.2 % |
| 4.2 % | 4.2 % |
Flexural Strength | 61.0 MPa | 8850 psi |
Flexural Modulus | 1.822 GPa | 264.3 ksi |
Izod Impact, Notched (ISO) | 5.20 kJ/m² @Temperature -30.0 °C | 2.47 ft-lb/in² @Temperature -22.0 °F |
| 5.20 kJ/m² @Temperature 0.000 °C | 2.47 ft-lb/in² @Temperature 32.0 °F |
| 5.20 kJ/m² @Temperature 23.0 °C | 2.47 ft-lb/in² @Temperature 73.4 °F |
Izod Impact, Unnotched (ISO) | NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
| NB @Temperature 0.000 °C | NB @Temperature 32.0 °F |
| NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
Puncture Energy | 43.0 J | 31.7 ft-lb |
|
Thermal Properties | Metric | English | Comments |
---|
Vicat Softening Point | 79.0 °C | 174 °F |
Glass Transition Temp, Tg | 85.0 °C | 185 °F |
|
Optical Properties | Metric | English | Comments |
---|
Haze | <= 1.0 % @Thickness 5.00 mm | <= 1.0 % @Thickness 0.197 in |
Gloss | 166 % | 166 % |
Yellow Index | <= 1.0 % @Thickness 5.00 mm | <= 1.0 % @Thickness 0.197 in |
Transmission, Visible | 60 % @Thickness 6.00 mm, Wavelength 400 nm | 60 % @Thickness 0.236 in, Wavelength 400 nm |
| 63 % @Thickness 5.00 mm, Wavelength 400 nm | 63 % @Thickness 0.197 in, Wavelength 400 nm |
| 69 % @Thickness 4.00 mm, Wavelength 400 nm | 69 % @Thickness 0.157 in, Wavelength 400 nm |
| 71 % @Thickness 3.00 mm, Wavelength 400 nm | 71 % @Thickness 0.118 in, Wavelength 400 nm |
| 77 % @Thickness 2.00 mm, Wavelength 400 nm | 77 % @Thickness 0.0787 in, Wavelength 400 nm |
| 81 % @Thickness 6.00 mm, Wavelength 440 nm | 81 % @Thickness 0.236 in, Wavelength 440 nm |
| 83 % @Thickness 5.00 mm, Wavelength 440 nm | 83 % @Thickness 0.197 in, Wavelength 440 nm |
| 84 % @Thickness 1.00 mm, Wavelength 400 nm | 84 % @Thickness 0.0394 in, Wavelength 400 nm |
| 85 % @Thickness 4.00 mm, Wavelength 440 nm | 85 % @Thickness 0.157 in, Wavelength 440 nm |
| 86 % @Thickness 3.00 mm, Wavelength 440 nm | 86 % @Thickness 0.118 in, Wavelength 440 nm |
| 87 % @Thickness 5.00 mm, Wavelength 590 nm | 87 % @Thickness 0.197 in, Wavelength 590 nm |
| 87.5 % @Thickness 6.00 mm, Wavelength 590 nm | 87.5 % @Thickness 0.236 in, Wavelength 590 nm |
| 88 % @Thickness 3.00 mm, Wavelength 590 nm | 88 % @Thickness 0.118 in, Wavelength 590 nm |
| 88 % @Thickness 2.00 mm, Wavelength 440 nm | 88 % @Thickness 0.0787 in, Wavelength 440 nm |
| 88.5 % @Thickness 4.00 mm, Wavelength 590 nm | 88.5 % @Thickness 0.157 in, Wavelength 590 nm |
| 89 % @Thickness 1.00 mm, Wavelength 590 nm | 89 % @Thickness 0.0394 in, Wavelength 590 nm |
| 89 % @Thickness 1.00 mm, Wavelength 440 nm | 89 % @Thickness 0.0394 in, Wavelength 440 nm |
| 89.5 % @Thickness 2.00 mm, Wavelength 590 nm | 89.5 % @Thickness 0.0787 in, Wavelength 590 nm |
| 90 % @Thickness 4.00 - 6.00 mm, Wavelength 700 nm | 90 % @Thickness 0.157 - 0.236 in, Wavelength 700 nm |
| 91 % @Thickness 1.00 - 3.00 mm, Wavelength 700 nm | 91 % @Thickness 0.0394 - 0.118 in, Wavelength 700 nm |
UV Transmittance | 45 % @Thickness 6.00 mm, Wavelength 370 nm | 45 % @Thickness 0.236 in, Wavelength 370 nm |
| 50 % @Thickness 5.00 mm, Wavelength 370 nm | 50 % @Thickness 0.197 in, Wavelength 370 nm |
| 58 % @Thickness 4.00 mm, Wavelength 370 nm | 58 % @Thickness 0.157 in, Wavelength 370 nm |
| 61 % @Thickness 3.00 mm, Wavelength 370 nm | 61 % @Thickness 0.118 in, Wavelength 370 nm |
| 70 % @Thickness 2.00 mm, Wavelength 370 nm | 70 % @Thickness 0.0787 in, Wavelength 370 nm |
| 80 % @Thickness 1.00 mm, Wavelength 370 nm | 80 % @Thickness 0.0394 in, Wavelength 370 nm |
|
Processing Properties | Metric | English | Comments |
---|
Melt Temperature | 180 - 250 °C | 356 - 482 °F |
Drying Temperature | <= 70.0 °C | <= 158 °F |
| 60.0 - 65.0 °C @Time 21600 - 28800 sec | 140 - 149 °F @Time 6.00 - 8.00 hour |
Moisture Content | <= 0.0040 % | <= 0.0040 % |
Dew Point | -40.0 °C | -40.0 °F |
|
Descriptive Properties |
---|
Particle size | 320 ± 50 mg/20 chips |
Pellet Shape | Cylindrical |