MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Pressure Seal 9727 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 9727 is a 70 durometer brown colored general purpose Fluorinated Hydrocarbon elastomer. It exhibits good resistance to heat, compression set, petroleum based oils, aliphatic and aromatic fuels.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 715 A1-10 B37 B38 EF31 EO78; 4 HK 715 A1-11 B38 EF31 EO78; 6 HK 715 A1-10 A1-11 B31 EF31 EO88
This Compound is RoHS Compliant

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.07 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 72
 60
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 67
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 68
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 69
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 70
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 70
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 72
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 73
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 75
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
Tensile Strength 1662 psi
 1178.4 psi
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 1204.9 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 1332.9 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 1459.2 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 1648.7 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 1675.3 psi
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 1760.1 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 1864.8 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
Elongation, Ultimate 220 %
 200 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 210.1 %
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 220 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 229.9 %
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 229.9 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 229.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 240 %
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 240 %
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
100% Modulus 753 psi
Tear Strength 220 pliDie B
Compression Set 9.2 %
@Treatment Temp. 175 °C,
Time 79200 sec
Plied
 13.2 %
@Treatment Temp. 23.0 °C,
Time 79200 sec
Plied
 16.7 %
@Treatment Temp. 200 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -8.00 °F
Shrinkage -0.200 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 0.30 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 1.5 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 3.5 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 4.4 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 8.5 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Service Fluid 100
 16 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Stauffer Blend 7700
 
Descriptive Properties
ColorBrown

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL120 / 318330

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.