MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Pressure Seal 8703 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 8703 is a 70 durometer black colored Viton® GLT. It exhibits good low temperature flexibility coupled with good heat, fluid and compression set resistance.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 720 A1-10 B37 B38 EF31 F15; 4 HK 720 A1-11 B38 EF31 EO78 F17; 6 HK 720 A1-10 A1-11 B31 B38 EF31 EO88 F15
AMS-R-83485 Type I
This Compound is RoHS Compliant

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.84 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 70
 62
@Treatment Temp. 23.0 °C,
Time 605000 sec
15% EtOH/85% FUEL C
 63
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
15% EtOH/85% FUEL C
 64
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 64
@Treatment Temp. 23.0 °C,
Time 252000 sec
15% EtOH/85% FUEL C
 64
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
15% EtOH/85% FUEL C
 65
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 65
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
85% EtOH/15% FUEL C
 65
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
85% EtOH/15% FUEL C
 66
@Treatment Temp. 23.0 °C,
Time 605000 sec
85% EtOH/15% FUEL C
 67
@Treatment Temp. 23.0 °C,
Time 605000 sec
Ethanol
 67
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
Ethanol
 67
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
Ethanol
 67
@Treatment Temp. 23.0 °C,
Time 252000 sec
85% EtOH/15% FUEL C
 68
@Treatment Temp. 23.0 °C,
Time 252000 sec
Ethanol
 69
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 70
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 70
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 71
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 71
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 72
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
Tensile Strength 2439 psi
 1761 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 1917.1 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 2051.2 psi
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 2304.9 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 2387.8 psi
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 2409.7 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 2431.7 psi
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
 2439 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
Elongation, Ultimate 273 %
 209.7 %
@Treatment Temp. 200 °C,
Time 252000 sec
Service Fluid 101
 233.4 %
@Treatment Temp. 200 °C,
Time 252000 sec
Stauffer Blend 7700
 234 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 249 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 264.8 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 270.5 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 313.7 %
@Treatment Temp. 275 °C,
Time 252000 sec
Heat Aged
 458.6 %
@Treatment Temp. 250 °C,
Time 252000 sec
Heat Aged
100% Modulus 576 psi
Tear Strength 126 pliDie C
 137 pliDie B
Compression Set 10 %
@Treatment Temp. 175 °C,
Time 79200 sec
Plied
 10.2 %
@Treatment Temp. 23.0 °C,
Time 79200 sec
Plied
 11.8 %
@Treatment Temp. 200 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -48.0 °F
Shrinkage 0.40 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 0.40 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 1.7 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 3.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Ethanol
 5.0 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 6.2 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, 85% EtOH/15% FUEL C
 6.2 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
Volume, Ethanol
 9.5 %
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
Volume, Ethanol
 9.5 %
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
Volume, Ethanol
 9.9 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
Volume, 85% EtOH/15% FUEL C
 9.9 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Service Fluid 100
 12.8 %
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
Volume, 85% EtOH/15% FUEL C
 13 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, 15% EtOH/85% FUEL C
 13.3 %
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
Volume, 85% EtOH/15% FUEL C
 15.8 %
@Treatment Temp. 200 °C,
Time 252000 sec
Volume, Stauffer Blend 7700
 18.7 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
Volume, 15% EtOH/85% FUEL C
 19.2 %
@Treatment Temp. 23.0 °C,
Time 5.76e+6 sec
Volume, 15% EtOH/85% FUEL C
 19.3 %
@Treatment Temp. 23.0 °C,
Time 2.16e+6 sec
Volume, 15% EtOH/85% FUEL C
 
Descriptive Properties
ColorBlack
TR-10 Temperature-34°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL100 / 318310

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.