MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Wieland Auropal 2 Casting Alloy
Categories: Metal; Nonferrous Metal; Precious Metal; Gold Alloy; Silver Alloy

Material Notes: Gold-silver casting alloy

Applications: inlays/onlays, crowns, short span bridges, long span bridges, telescopic and milling works, removable partials, acrylic veneering

Dental

Key Words: EN ISO 8891
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 13.8 g/cc0.499 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 270270HV5/30; as cast
 280280HV5/30; hardened
Tensile Strength, Yield  320.00 MPa
@Strain 0.2 %
46412 psi
@Strain 0.2 %
as cast
 660.00 MPa
@Strain 0.2 %
95725 psi
@Strain 0.2 %
hardened
Elongation at Break 8.0 %8.0 %hardened
 35 %35 %as cast
Modulus of Elasticity 104 GPa15100 ksi
 
Thermal PropertiesMetricEnglishComments
Melting Point 899 - 960 °C1650 - 1760 °F
Solidus 899 °C1650 °F
Liquidus 960 °C1760 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 699 °C1290 °FPreheating Temp.
Casting Temperature 1110 °C2030 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 11.5 %11.5 %
Gold, Au 55 %55 %
Iridium, Ir 0.10 %0.10 %
Palladium, Pd 7.9 %7.9 %
Silver, Ag 25 %25 %
Zinc, Zn 0.50 %0.50 %
 
Descriptive Properties
Coloryellow

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
HGC-4 Precious dental alloy
Gold, Au; 18K, Yellow (UNS P00255)
HGC-1 Precious dental alloy
Wieland 1401 Wilaform Gold
Wieland Auropal 1 Casting Alloy

NWIELAN26 / 19828

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.