MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

EMS-Grivory Grilamid® L 25 W 40 NZ PA12-I
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: Product Description: Grilamid L 25 W 40 NZ is a flexible, plasticized, high viscosity extrusion grade of Polyamide 12 (PA12). Grilamid L 25 W 40 NZ is impact modified and heat and UV stabilized. The main features of Grilamid L 25 W 40 NZ are:
  • Exceptional impact strength, also at low temperatures
  • Flexibility
  • UV and heat stability
  • Low density, low weight
  • Easy processing
Application examples: Grilamid L 25 W 40 NZ is suitable for the production of flexible tubes and profiles requiring good low temperature impact strength for use in automotive and industrial applications.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.00 g/cc0.0361 lb/in³Dry; ISO 1183
Water Absorption 1.4 %1.4 %Sim. to ISO 62
Moisture Absorption 0.700 %0.700 %Sim. to ISO 62
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 25.0 MPa3630 psiConditioned; ISO 2039-1
Tensile Strength at Break 30.0 MPa4350 psiConditioned; ISO 527-1/-2
 45.0 MPa6530 psiDry; ISO 527-1/-2
Tensile Strength, Yield 20.0 MPa2900 psiConditioned; ISO 527-1/-2
Elongation at Break >= 50 %>= 50 %Nominal, Conditioned; ISO 527-1/-2
 >= 50 %>= 50 %Dry; ISO 527-1/-2
Elongation at Yield 45 %45 %Conditioned; ISO 527-1/-2
Tensile Modulus 0.250 GPa36.3 ksiConditioned; ISO 527-1/-2
 0.300 GPa43.5 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  1.20 J/cm²
@Temperature -30.0 °C
5.71 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 1.30 J/cm²
@Temperature -30.0 °C
6.19 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+11 ohm-cm1.00e+11 ohm-cmConditioned; IEC 60093
Surface Resistance 1.00e+11 ohm1.00e+11 ohmIEC 60093
Dielectric Strength 32.0 kV/mm813 kV/inConditioned; IEC 60243-1
Comparative Tracking Index 600 V600 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 173 °C343 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 80.0 °C176 °FLong Term; ISO 2578
 110 °C230 °FShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 50.0 °C122 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 40.0 °C104 °FISO 75-1/-2
 
Descriptive Properties
AdditivesPlasticizer
AutomotiveCompressed air systems
 Fuel systems
FormGranules
Industry & Consumer goodsHydraulics & Pneumatics
ProcessingOther Extrusion
Product AttributesFlexible
 High viscosity
Special CharacteristicsHigh impact or impact modified
 Improved heat resistance
 Improved UV resistance (outdoor use)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 12

PGRH053 / 156762

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.