MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Envalior Pocan® KU 1-7635 901510 PBT + PC, 30% Glass Fiber
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate/Polybutylene Terephthalate (PBT) Blend, Glass Filled; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: PBT+PC, 30% glass fibers, injection molding, low tendency to warp, improved surface finish

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.50 g/ccISO 1183
Water Absorption 0.30 %Test Sim. to ISO 62
Moisture Absorption at Equilibrium 0.10 %23°C/50% R.H.; Test Sim. to ISO 62
Melt Flow 18 g/10 min
@Load 2.16 kg,
Temperature 260 °C
Calculated from MVR using melt density; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 100 MPaISO 527-1/-2
Elongation at Break 2.5 %ISO 527-1/-2
Tensile Modulus 7500 MPaISO 527-1/-2
Charpy Impact Unnotched 50.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 150 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 30.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 80.0 µm/m-°CISO 11359-1/-2
Melting Point 225 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 165 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 120 °CISO 75-1/-2
Flammability, UL94 HB
@Thickness 0.800 mm
IEC 60695-11-10
 HB
@Thickness 1.60 mm
IEC 60695-11-10
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °CInjection Molding; ISO 294
Mold Temperature 80.0 °CInjection Molding; ISO 10724
 
Descriptive Properties
AdditivesRelease agent
FormPellets
ISO Short NameISO 7792-1-PBT+PC,GHMR,09-080,GF30
ProcessingInjection molding
RegionAsia Pacific
 Europe
 Near East/Africa
 North America
 South and Central America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Pocan® B 3235 901510 PBT, 30% Glass Fiber
Covestro Makrolon® RW 6267X Polycarbonate, 10% Glass Fiber
Envalior Pocan® KU 2-7604 000000 PBT+PC
Envalior Pocan® DP 7244 000000 PBT, 30% Glass Fiber
Envalior Pocan® BF 4222 000000 PBT, 20% Glass Fiber Reinforced

PLANX0895 / 99110

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.