MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

KKPC KOSYN SOL 5520 Solution Styrene Butadiene Rubber (S-SBR)
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Solution Styrene Butadiene Rubber (S-SBR)

Characteristics: This product is made by solution polymerization under which styrene and butadiene react in organic solvent using alkyl-lithium catalyst. It is superior to SBR, which is made by emulsion polymerization, in processability, visco-elasticity and low temperature properties. Also, the products' properties can be adjusted to the purpose of consumption according to the proper proportion of styrene content, the micro structure and the molecular weight.

Applications: Shoes, Soles, Tires, Machine Parts, Energy-saving Tires, High-efficiency Tires

Additional Notes:
Bound Styrene: 23.7%
cis-1,4 Contents: 25%
trans-1,4 Contents: 39%
Vinyl Contents: 39%
Dynamic Test: GABO Qualimeter (11Hz)
(TAN) 0°C: 0.326
10°C: 0.214
60°C: 0.125
70°C: 0.116

This product is so sensitive to sunlight and humidity that it can be tarnished and caused deterioration of quality if exposed. It is recommended to store it in cool and shady area lest it should be exposed to direct sunlight. Do not expose to incompatible materials or contaminants.

Data provided by Korea Kumho Petrochemical Co., Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Mooney Viscosity  54
@Temperature 100 °C
54
@Temperature 212 °F
Raw; ML1+4
 93
@Temperature 100 °C
93
@Temperature 212 °F
ML1+4; Polymer 100, HAF Black (IRB#6) 50, ZnO 3, Stearic Acid 1, D 0.3, DM 0.6, Sulfur 1.75, Total: 156.65, Cure: 145°C, 35 minutes.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6969JIS-A
Tensile Strength, Ultimate 27.3 MPa3950 psi
Elongation at Break 500 %500 %
300% Modulus 14.5 MPa
@Strain 300 %
2110 psi
@Strain 300 %
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg -34.0 °C-29.2 °FCompound

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
KKPC KOSYN SOL 5001 Solution Styrene Butadiene Rubber (S-SBR)
KKPC KOSYN SOL 5740 Solution Styrene Butadiene Rubber (S-SBR)
Synthos SPRINTAN™ SLR 4302-SCHKOPAU Solution-Styrene Butadiene Rubber (S-SBR)
Garlock 60 SBR Sheet Rubber
Garlock 50 Natural/SBR Sheet Rubber

PKKPC23 / 48754

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.