MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Cartridge Brass, UNS C26000 (260 Brass), H06 wire
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: Fair to excellent corrosion resistance. Excellent cold workability; good hot formability.

Applications: radiator cores and tanks, flashlight shells, lamp fixtures, fasteners, locks, hinges, ammunition components, plumbing accessories, pins, rivets.

Test specimen: wire - 2mm diameter.

Key Words: 70/30 brass, CDA 260, CZ106, ISO CuZn30, CEN CW505L
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.53 g/cc0.308 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 855 MPa124000 psi
Elongation at Break 4.0 %4.0 %in 50 mm
Modulus of Elasticity 110 GPa16000 ksi
Poissons Ratio 0.3750.375
Machinability 30 %30 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 40.0 GPa5800 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear 19.9 µm/m-°C
@Temperature 20.0 - 300 °C
11.1 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.375 J/g-°C0.0896 BTU/lb-°F
Thermal Conductivity 120 W/m-K
@Temperature 20.0 °C
833 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 915 - 955 °C1680 - 1750 °F
Solidus 915 °C1680 °F
Liquidus 955 °C1750 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 425 - 750 °C797 - 1380 °F
Hot-Working Temperature 725 - 850 °C1340 - 1560 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 68.5 - 71.5 %68.5 - 71.5 %
Iron, Fe <= 0.050 %<= 0.050 %
Lead, Pb <= 0.070 %<= 0.070 %
Other, total <= 0.15 %<= 0.15 %
Zinc, Zn >= 28.5 %>= 28.5 %
 
Descriptive Properties
Hall Coefficient48 pV · m/A · T
Velocity of Sound3660 m/sat 20°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Cartridge Brass, UNS C26000 (260 Brass), H00 Temper wire
Cartridge Brass, UNS C26000 (260 Brass), OS050 Temper wire
Cartridge Brass, UNS C26000 (260 Brass), H01 Temper wire
Cartridge Brass, UNS C26000 (260 Brass), H02 Temper rod
Cartridge Brass, UNS C26000 (260 Brass), H08 Temper wire

MC26000d7 / 11099

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.