MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

SABIC NORYL™ Resin BN31 Polyphenylene Ether + PS (PPE+PS) (Asia)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL™ BN31 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This blow moldable grade contains non-brominated, non-chlorinated flame retardant and carries a UL94 flame rating of 5VA at 2.5mm and V0 at 1.5mm along with a UL746C Outdoor Suitability rating of F1. NORYL BN31 resin exhibit good low temperature impact strength, heat resistance, excellent processability, Low warpage, and dimensional stability. The material is an excellent candidate for blow molded applications such as hospital bed headboard, cladding, tray.

Features: Hydrolytic Stability,Flame Retardant,Non-Halogenated,Low Warpage,High Impact Resistance,High Flow,Good Processability,Exceptional Processing

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.10 g/cc1.10 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0060 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0060 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 48.0 MPa6960 psi50 mm/min; ASTM D638
Flexural Strength 72.0 MPa10400 psibrk, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.41 GPa350 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 267 J197 ft-lbASTM D256
 106 J
@Temperature -40.0 °C
78.2 ft-lb
@Temperature -40.0 °F
ASTM D256
Gardner Impact 13.0 J9.59 ft-lbASTM D3029
 33.0 J
@Temperature -40.0 °C
24.3 ft-lb
@Temperature -40.0 °F
ASTM D3029
 
Electrical PropertiesMetricEnglishComments
Hot Wire Ignition, HWI 30 - 60 sec
@Thickness >=3.00 mm
30 - 60 sec
@Thickness >=0.118 in
UL 746A
High Amp Arc Ignition, HAI 30 - 60 arcs
@Thickness >=3.00 mm
30 - 60 arcs
@Thickness >=0.118 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR >= 150 mm/min>= 5.91 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 82.0 °C
@Thickness 6.40 mm
180 °F
@Thickness 0.252 in
unannealed; ASTM D648
UL RTI, Electrical 95.0 °C203 °FUL 746B
UL RTI, Mechanical with Impact 80.0 °C176 °FUL 746B
UL RTI, Mechanical without Impact 95.0 °C203 °FUL 746B
Flammability, UL94  V-0
@Thickness >=1.50 mm
V-0
@Thickness >=0.0591 in
UL 94
 5VA
@Thickness >=3.00 mm
5VA
@Thickness >=0.118 in
UL 94
 
Processing PropertiesMetricEnglishComments
Zone 1 205 - 215 °C401 - 419 °FExtrusion Blow Molding
Zone 2 205 - 215 °C401 - 419 °FExtrusion Blow Molding
Zone 3 205 - 215 °C401 - 419 °FExtrusion Blow Molding
Zone 4 210 - 215 °C410 - 419 °FExtrusion Blow Molding
Zone 5 210 - 215 °C410 - 419 °F
Die Temperature 215 - 220 °C419 - 428 °FExtrusion Blow Molding
Melt Temperature 210 - 215 °C410 - 419 °FExtrusion Blow Molding
Head Temperature 210 - 215 °C410 - 419 °FZone 6 - Top Temperature
 215 - 220 °C419 - 428 °FZone 7 - Bottom Temperature
Mold Temperature 50.0 - 70.0 °C122 - 158 °F
Drying Temperature 95.0 °C203 °FExtrusion Blow Molding
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourExtrusion Blow Molding
 
Descriptive Properties
UV-light, water exposure/immersionF1UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82256 / 290203

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.