MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 12L13 Steel, cold drawn, 19-38 mm round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: Applications include high-speed screw machine products where superior machining characteristics of this steel can be fully utilized.

Key Words: UNS G12134, ASTM A29, FED QQ-S-633(C12l13), MIL SPEC MIL-S-18411, SAE J403, JIS SUM 24 L, SS14 1914 (Sweden), SAE J412, DIN 1.0718, UNI 9SMnPb23, JIS SUM 22 L, JIS SUM 23 L
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.87 g/ccTypical For Steel
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 163(AISI 12L14)
Hardness, Knoop 184Converted from Brinell
Hardness, Rockwell B 84Converted from Brinell
Hardness, Vickers 170Converted from Brinell
Tensile Strength, Ultimate 540 MPa(AISI 12L14)
Tensile Strength, Yield 415 MPa(AISI 12L14)
Elongation at Break 10 %(AISI 12L14)
Reduction of Area 35 %(AISI 12L14)
Modulus of Elasticity 200 GPaTypical For Steel
Bulk Modulus 160 GPaTypical For Steel
Poissons Ratio 0.29Typical For Steel
Machinability 160 %(AISI 12L14) Based on 100% machinability for AISI 1212 steel.
Shear Modulus 80.0 GPaTypical For Steel
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000174 ohm-cmTypical For Steel
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.5 µm/m-°C
@Temperature 20.0 °C
Typical For Steel
 12.2 µm/m-°C
@Temperature 0.000 - 300 °C
Typical For Steel
 13.9 µm/m-°C
@Temperature 0.000 - 500 °C
Typical For Steel
Specific Heat Capacity 0.472 J/g-°CTypical For Steel
Thermal Conductivity 51.9 W/m-KTypical For Steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.13 %
Iron, Fe 98.07 - 98.84 %As remainder
Lead, Pb 0.15 - 0.35 %
Manganese, Mn 0.70 - 1.0 %
Phosphorus, P 0.070 - 0.12 %
Sulfur, S 0.24 - 0.33 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 12L13 Steel, hot rolled, 19-38 mm round
AISI 12L14 Steel, cold drawn, 19-38 mm round
AISI 1213 Steel, hot rolled, 19-38 mm round
AISI 1213 Steel, cold drawn, 19-38 mm round
AISI 12L14 Steel, hot rolled, 19-38 mm round

M121EA2 / 7312

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.