MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SEKISUI SPI ALLEN® 8300FR PC/ABS Sheet
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced

Material Notes: ALLEN® 8300FR is a polycarbonate and ABS blend with high impact properties, stiffness, heat resistance, and a non-halogenated flame retardant V-0 @ 0.060”, 5VA @ 0.118” rating.

ALLEN® 8300FR has been tested under laboratory conditions and has achieved a UL94 V-0 rating at 0.060 in (1.52mm) and above and meets the requirements of Federal Motor Vehicle Safety Standard No. 302 (FMVSS 302).

Suggested Application:

  • Medical Equipment Housings
  • Electrical Housings and Covers
  • Vehicle Interior Trim Parts
  • Battery Charging Station
Features:
  • Flame retardant
  • Halogen free
  • Low smoke toxicity
  • High heat deflection temperature
  • Increased stiffness
  • Edge trim easily used into future orders
  • High gloss finish

Information provided by SEKISUI KYDEX, LLC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.21 g/ccASTM D792
Water Absorption 0.140 %
@Time 86400 sec
ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 119ASTM D785
Tensile Strength 65.1 MPaASTM D638
Tensile Modulus 2630 MPaASTM D638
Flexural Strength 100.7 MPa
@Strain 5.00 %
ASTM D790
Flexural Modulus 2630 MPaASTM D790
Compressive Yield Strength 80.7 MPaASTM D695
Bearing Yield Strength <= 293 MPaASTM D953
 29.5 MPa
@Strain 4.00 %
ASTM D953
Shear Strength 61.9 MPaASTM D732
Izod Impact, Notched 640.8 J/mASTM D256
Gardner Impact 68.4 JDrop Dart Impact, GE; ASTM D5420
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 16.7 kV/mmoil; ASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 68.0 µm/m-°CASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 112 °Cannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 109 °Cannealed; ASTM D648
Flammability, UL94 V-0
@Thickness 1.52 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSEKIS523 / 325263

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.