MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Magnesium
Magnesium Elektron - Service & Innovation in Magnesium

(Viewing data as-entered. Click here to return)
Magnesium Elektron Elektron® 43 Magnesium Wrought Alloy
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes: High strength wrought Mg alloy available as rolled plate, forging feedstock, and extrusions. It is a wrought evolution of the casting alloy Elektron WE43. Elektron 43 uses zirconium grain refining and has successfully undergone flammability tests by the FAA for use in aircraft seat frames. It develops maximum strength in the T5 condition.

Vendors: Magnesium Elektron is the world leader in high strength magnesium alloys in rolled, extruded and cast forms. Phone (303) 589-3189 or visit www.magnesium-elektron.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.84 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 70 - 90
Tensile Strength 43.0 ksiExtruded Bar - Transverse
 48.0 ksiExtruded Bar - Longitudinal
 50.0 ksi
@Thickness 1.02 - 38.1 mm
Rolled Plate
 50.0 ksi
@Thickness 38.13 - 76.2 mm
Rolled Plate
Tensile Strength, Yield 26.0 ksi
@Strain 0.2 %
Extruded Bar - Transverse
 31.0 ksi
@Strain 0.2 %
Extruded Bar - Longitudinal
 37.0 ksi
@Strain 0.2 %,
Thickness 38.13 - 76.2 mm
Rolled Plate
 40.0 ksi
@Strain 0.2 %,
Thickness 1.02 - 38.1 mm
Rolled Plate
Elongation at Break 11 %Extruded Bar - Transverse
 14 %Extruded Bar - Longitudinal
 12 %
@Thickness 1.02 - 38.1 mm
Rolled Plate
 14 %
@Thickness 38.13 - 76.2 mm
Rolled Plate
Modulus of Elasticity 44.0 GPa
Poissons Ratio 0.27
Fatigue Strength 27000 psi
@# of Cycles 5.00e+7
Axial; R = 0.1; Extruded Bar; ASTM E466
Shear Modulus 17.3 GPaCalculated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000148 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 26.7 µm/m-°C
 26.7 µm/m-°C
Specific Heat Capacity 0.966 J/g-°C
Thermal Conductivity 51.3 W/m-K
Melting Point 540 - 640 °C
Solidus 540 °C
Liquidus 640 °C
Maximum Service Temperature, Air 480 °F
 
Component Elements PropertiesOriginal ValueComments
Magnesium, Mg 92 - 93.8 %as balance
Rare Earths 2.3 - 3.5 %
Yttrium, Y 3.7 - 4.3 %
Zirconium, Zr >= 0.20 %
 
Descriptive Properties
Damping Index0.09

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Magnesium Elektron Elektron® 675 Magnesium Wrought Alloy
Magnesium Elektron Elektron® 43 Magnesium Extrusion Alloy, UNS M18434
Magnesium Elektron Elektron® 21 Magnesium Casting Alloy
Magnesium EA55RS-T4, Extruded
Alclad Aluminum 2024-T4, T351

NMAGEL899 / 147648

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.