MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ATI Wah Chang Zirconium Alloy Zircaloy-4
Categories: Metal; Nonferrous Metal; Zirconium Alloy

Material Notes: Zirconium resists corrosive attack in most organic and mineral acids, strong alkalis, and some molten salts. A tightly adherent and protective oxide film protects the metal-oxide interface to provide corrosion resistance. An additional benefit for zirconium alloys in long-term geological disposal options is the inert nature of zirconium oxide.

Information provided by ATI Wah Chang

Key Words: UNS R60804
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 0.237 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 89
Tensile Strength, Ultimate 34900 psi
@Temperature 288 °C
Transverse
 39300 psi
@Temperature 288 °C
Longitudinal
 74600 psi
@Temperature 23.0 °C
 78400 psi
@Temperature 23.0 °C
Tensile Strength, Yield 22000 psi
@Temperature 288 °C
Longitudinal
 25600 psi
@Temperature 288 °C
Transverse
 55200 psi
@Temperature 23.0 °C
 67800 psi
@Temperature 23.0 °C
Modulus of Elasticity 99.3 GPa
Poissons Ratio 0.37
Shear Modulus 5249 ksi
 
Thermal PropertiesOriginal ValueComments
CTE, linear 6.00 µm/m-°C
@Temperature 20.0 °C
Thermal Conductivity 149 BTU-in/hr-ft²-°F
Melting Point 1850 °C
 
Component Elements PropertiesOriginal ValueComments
Chromium, Cr 0.070 - 0.13 %
Fe + Cr 0.28 - 0.37 %
Iron, Fe 0.18 - 0.24 %
Tin, Sn 1.2 - 1.7 %
Zirconium, Zr 97.56 - 98.27 %
 
Descriptive Properties
Alpha + Beta -> Beta Phase Transformation980°C
Alpha -> Alpha + Beta Phase Transformation810°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Zircaloy-4 Zirconium Alloy
Zircaloy-2 Zirconium Alloy
Grade 706 Zirconium (Zr-2.5Nb)
Reactor Grade Zirconium
Zr-2.5Nb Zirconium Alloy, Nuclear Grade

NATIWC20 / 15075

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.