MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Avient OnFlex™ BIO 5370A-E0004 Thermoplastic Elastomer (TPE)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Elastomer, TPE

Material Notes: OnFlex™-Bio 5300 series thermoplastic elastomer compounds are soft thermoplastic polyurethane compounds made from renewable natural sources. These compounds contain at least 20% of renewable material as certified according to ASTM-D6866. The OnFlex™-Bio 5300 series compounds are formulated to provide an excellent surface finish, soft-touch haptic, abrasion resistance and mechanical properties.

Properties are measured using injection molded plaques.

Information provided by PolyOne

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 70ISO 868
Tensile Strength at Break 11.0 MPa
@Thickness 2.00 mm,
Temperature 23.0 °C
Type 1, 200 mm/min Across Flow; DIN 53504
 12.7 MPa
@Thickness 2.00 mm,
Temperature 23.0 °C
Type 1, 200 mm/min; Flow; DIN 53504
Tensile Stress at Strain 3.30 MPa
@Strain 100 %,
Thickness 2.00 mm
Type 1, 200 mm/min Across Flow; DIN 53504
 3.80 MPa
@Strain 100 %,
Thickness 2.00 mm
Type 1, 200 mm/min; Flow; DIN 53504
 7.90 MPa
@Strain 300 %,
Thickness 2.00 mm
Type 1, 200 mm/min Across Flow; DIN 53504
 9.20 MPa
@Strain 300 %,
Thickness 2.00 mm
Type 1, 200 mm/min; Flow; DIN 53504
Elongation at Break 410 %
@Thickness 2.00 mm,
Temperature 23.0 °C
Type 1, 200 mm/min Across Flow; DIN 53504
 410 %
@Thickness 2.00 mm,
Temperature 23.0 °C
Type 1, 200 mm/min; Flow; DIN 53504
Tear Strength 43.0 kN/m
@Thickness 2.00 mm,
Temperature 23.0 °C
Method A, Trouser; Across Flow; ISO 34-1
 47.0 kN/m
@Thickness 2.00 mm,
Temperature 23.0 °C
Method A, Trouser; Flow; ISO 34-1
Abrasion 63[mm³]; DIN 53516
Compression Set 51 %
@Temperature 23.0 °C,
Time 259000 sec
ISO 815
 73 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 84 %
@Temperature 100 °C,
Time 79200 sec
ISO 815
 
Processing PropertiesOriginal ValueComments
Melt Temperature 180 - 220 °C
Mold Temperature 30.0 - 60.0 °C
Drying Temperature 100 - 120 °C
Dry Time 1.00 - 2.00 hour
 
Descriptive Properties
FeaturesGood Abrasion Resistance
 Renewable Resource Content
 Scratch Resistant
FormsPellets
Generic MaterialTPE
Generic NameThermoplastic Elastomer (TPE)
Injection RateFast
Odor rating3VDA 270; Method A3
Processing MethodCalendering
 Extrusion
 Injection Molding
 Multi Injection Molding
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
RoHS ComplianceRoHS Compliant
UsesAutomotive Applications
 Consumer Applications
 General Purpose

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Avient Dynaflex™ G7930-1001-00 Thermoplastic Elastomer (TPE)
Avient OnFlex™ S HF 60A-3S1982 Thermoplastic Elastomer (TPE)
Avient OnFlex™ S HS 70A-3E2543 Thermoplastic Elastomer (TPE)
Avient OnFlex™ S KE 60A-3S1725 Thermoplastic Elastomer (TPE)
Avient Versaflex™ HC 2110-57B Thermoplastic Elastomer (TPE)

PH0POL1030 / 145599

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.