MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 8090-T852
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Other Wrought Al Alloy

Material Notes: Common heat treatment for die forgings with cold work and hand forgings.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 8090-T852; AlLi; Aluminum Lithium Alloy; AA8090-T852; UNS A98090; Al8090-T852
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.54 g/cc0.0918 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 128128500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 161161Converted from Brinell Hardness Value
Hardness, Rockwell A 48.948.9Converted from Brinell Hardness Value
Hardness, Rockwell B 7979Converted from Brinell Hardness Value
Hardness, Vickers 146146Converted from Brinell Hardness Value
Tensile Strength, Ultimate 480 MPa69600 psi
Tensile Strength, Yield 410 MPa59500 psi
Elongation at Break 7.0 %7.0 %In 5 cm
Modulus of Elasticity 77.0 GPa11200 ksi
Fracture Toughness 15.0 MPa-m½13.7 ksi-in½K(IC) in S-L Direction
 20.0 MPa-m½18.2 ksi-in½K(IC) in T-L Direction
 30.0 MPa-m½27.3 ksi-in½K(IC) in L-T Direction
Shear Strength 280 MPa40600 psiCalculated value.
 
Thermal PropertiesMetricEnglishComments
CTE, linear 21.4 µm/m-°C
@Temperature 20.0 - 100 °C
11.9 µin/in-°F
@Temperature 68.0 - 212 °F
Specific Heat Capacity 0.930 J/g-°C
@Temperature 100 °C
0.222 BTU/lb-°F
@Temperature 212 °F
Thermal Conductivity 95.3 W/m-K661 BTU-in/hr-ft²-°F
Melting Point 600 - 655 °C1110 - 1210 °F
Solidus 600 °C1110 °F
Liquidus 655 °C1210 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 93 - 96.2 %93 - 96.2 %As remainder
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu 1.0 - 1.6 %1.0 - 1.6 %
Iron, Fe <= 0.30 %<= 0.30 %
Lithium, Li 2.2 - 2.7 %2.2 - 2.7 %
Magnesium, Mg 0.60 - 1.3 %0.60 - 1.3 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.20 %<= 0.20 %
Titanium, Ti <= 0.10 %<= 0.10 %
Zinc, Zn <= 0.25 %<= 0.25 %
Zirconium, Zr 0.04 - 0.16 %0.04 - 0.16 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 8090-T81
Aluminum 8090-T8x
Aluminum 8090-T8151
Aluminum 8090-T511 and 8090-T6511
Aluminum 8090-T3

MA8090T852 / 9698

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.