MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

SABIC NORYL™ Resin PKN4752 Polyphenylene Ether + PS (PPE+PS) (Europe)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL PKN4752 resin is a non-reinforced, translucent, high heat blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This extrudable and injection moldable grade exhibits high heat resistance, dimensional stability, and appears translucent with a yellow tint in the natural color. NORYL PKN4752 resin is an excellent candidate for high performance packaging in food, electronics, and healthcare. *See NORYL PKN4752F resin for FDA food compliant version.

Features: Hydrolytic Stability,Low Creep Sensitivity,High Heat Resistance,Translucent,Low Warpage

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.08 g/cc0.0390 lb/in³ISO 1183
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 86.0 MPa12500 psi50 mm/min; ISO 527
Elongation at Break 6.0 %6.0 %50 mm/min; ISO 527
Tensile Modulus 3.10 GPa450 ksi1 mm/min; ISO 527
Flexural Strength 130 MPa18900 psiyield, 2 mm/min; ISO 178
Flexural Modulus 2.95 GPa428 ksi2 mm/min; ISO 178
Izod Impact, Notched (ISO) 3.00 kJ/m²1.43 ft-lb/in²80*10*4; ISO 180/1A
 3.00 kJ/m²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 0.200 J/cm²0.952 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 0.200 J/cm²
@Temperature -30.0 °C
0.952 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 163 °C325 °FEdgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi) 147 °C297 °FEdgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point 174 °C345 °FRate A/50; ISO 306
 
Processing PropertiesMetricEnglishComments
Processing Temperature 60.0 - 80.0 °C140 - 176 °FCalibrator Temperature
Zone 1 215 - 240 °C419 - 464 °FProfile Extrusion
Zone 2 225 - 250 °C437 - 482 °FProfile Extrusion
Zone 3 250 - 275 °C482 - 527 °FProfile Extrusion
Zone 4 250 - 275 °C482 - 527 °FProfile Extrusion
Adapter Temperature 250 - 275 °C482 - 527 °FProfile Extrusion
Die Temperature 250 - 275 °C482 - 527 °FProfile Extrusion
Melt Temperature 280 - 300 °C536 - 572 °FProfile Extrusion
Drying Temperature 80.0 - 95.0 °C176 - 203 °FProfile Extrusion
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourProfile Extrusion
Precipitation Temperature 50.0 - 70.0 °C122 - 158 °FHopper Temperature

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82416 / 290363

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.