MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Braskem IN34 LLDPE Injection Molding Polyethylene Copolymer  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Extrusion Grade; LLDPE/Octene, Extruded; LLDPE/Hexene, Molded

Material Notes: IN34 is a linear low-density polyethylene, narrow molecular weight butene-1 copolymer produced by the solution process for injection molding applications. It offers high fluidity, excellent flexibility, and low warpage. It was specially developed for lids fast-cycle molding injection, natural color and dyed for food. It is also recommended for the food market. IN34 was developed to be injected in similar conditions to low-density polyethylene of similar fluidity. Recommended temperature profile: 170º to 210 ºC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.939 g/ccASTM-D729
Melt Flow 48 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM-D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 54ASTM-D2240
Tensile Strength at Break 10.0 MPaASTM-D638
Tensile Strength, Yield 19.0 MPaASTM-D638
Elongation at Break 100 %ASTM-D638
Elongation at Yield 12 %ASTM-D638
Modulus of Rigidity 0.645 GPaASTM-D747
Flexural Modulus, 1% Secant 640 MPaASTM-D790
Izod Impact, Notched 70.0 J/mASTM-D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 49.0 °CASTM-D648
Vicat Softening Point 100 °C
@Load 1.02 kg
ASTM-D1525

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Braskem IJ33D LLDPE Injection Molding Polyethylene Copolymer
Braskem IF33 LLDPE Injection Molding Polyethylene Copolymer
Braskem IC32 LLDPE Injection Molding Polyethylene Copolymer
Braskem ML2400N LLDPE Injection Molding Polyethylene
LyondellBasell Petrothene GA574200 Linear Low Density Polyethylene (LLDPE), Injection Molded

PBRAS911 / 106757

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.