MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Beryllium-Copper Alloy 20C, UNS C82500, As Cast
Categories: Metal; Nonferrous Metal; Beryllium Alloy; Copper Alloy; Copper Casting Alloy

Material Notes:

Casting methods recommended for this alloy: Centrifugal, Investment, Permanent Mold, Plaster, and Sand.

Applications: Safety tools, molds for plastic parts, cams, bushings, valves, pump parts, and gears.

Test specimen: as cast.

Key Words: BeCu; beryllium copper 20C, standard beryllium copper casting alloy, CA 825, AMS 4890 (investment castings), FED QQ-C-390 (sand and centrifugal castings), MIL SPEC MIL-C-19464 (Class 2) sand castings, MIL-C-11866 (composition 17) and MIL-C-17324 precision castings, MIL-C-22087 investment castings, ICI-Cu-2-10780
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.26 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 81
Tensile Strength, Ultimate 515 MPa
Tensile Strength, Yield 275 MPa
@Strain 0.2 %
Elongation at Break 15 %In 50 mm
Modulus of Elasticity 128 GPa
Compressive Yield Strength 1030 - 1200 MPaPermanent set of 0.1%
Poissons Ratio 0.30
Fatigue Strength 165 MPa
@# of Cycles 5.00e+7
rotating beam; Temper Not Reported
Machinability 30 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 50.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000862 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.0 µm/m-°C
@Temperature 20.0 - 200 °C
Specific Heat Capacity 0.420 J/g-°C
Thermal Conductivity 105 W/m-K
@Temperature 20.0 °C
Melting Point 835 °CIncipient
 850 - 980 °C
Solidus 855 °C
Liquidus 980 °C
Shrinkage 1.56 %Patternmaker's Shrinkage (3/16 in./ft.)
 
Processing PropertiesOriginal ValueComments
Solution Temperature 790 - 800 °C
Aging Temperature 345 °C
Casting Temperature 1010 - 1065 °CHeavy castings
 1065 - 1175 °CLight castings
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al <= 0.15 %
Beryllium, Be 1.9 - 2.15 %
Chromium, Cr <= 0.10 %
Cobalt, Co 0.35 - 0.70 %
Copper, Cu >= 95.5 %
Iron, Fe <= 0.25 %
Lead, Pb <= 0.020 %
Nickel, Ni <= 0.20 %
Silicon, Si 0.20 - 0.35 %
Tin, Sn <= 0.10 %
Zinc, Zn <= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Beryllium-Copper Alloy 30C, UNS C82200, As-Cast
Beryllium-Copper Alloy 165C, UNS C82400, As-Cast
Beryllium-Copper Alloy 50C, UNS C81800, As-cast
Beryllium Copper Alloy 10C, UNS C82000 As-cast
Copper, Cu; Annealed

MC82500b2 / 11884

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.