MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Constellium ALPLAN® 2017A High-Strength Rolled Precision Aluminum Plate, Milled Both Sides
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: ALPLAN® 2017A precision plates combine a very good dimensional stability with a high level of mechanical strength and elongation. The outstanding flatness, the low roughness and high quality of the milled surfaces, protected by a plastic film, make surface milling by the end user superfluous. This combination of properties enables significant cost savings in machining. Applications include: reference plates, machine housings and lateral panels, transport tables, jigs.

Information provided by manufacturer

Key Words: EN AW-2017A T451
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.78 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 125
@Thickness 7.90 - 25.0 mm
 125
@Thickness 25.0 - 60.0 mm
 125
@Thickness 60.0 - 155 mm
Tensile Strength >= 370 MPa
@Thickness 60.0 - 80.0 mm
Temper T451; Standard EN 485-2
 >= 385 MPa
@Thickness 40.0 - 60.0 mm
Temper T451; Standard EN 485-2
 >= 390 MPa
@Thickness 7.90 - 12.5 mm
Temper T451; Standard EN 485-2
 >= 390 MPa
@Thickness 12.5 - 40.0 mm
Temper T451; Standard EN 485-2
 415 MPa
@Thickness 7.90 - 25.0 mm
Typical Strength; Standard EN 485-2
 415 MPa
@Thickness 25.0 - 60.0 mm
Typical Strength; Standard EN 485-2
 415 MPa
@Thickness 60.0 - 155 mm
Typical Strength; Standard EN 485-2
 >= 495 MPa
@Thickness 80.0 - 115 mm
Temper T451; Standard EN 485-2
Tensile Strength, Yield >= 240 MPa
@Strain 0.2 %,
Thickness 60.0 - 80.0 mm
Temper T451; Standard EN 485-2
 >= 245 MPa
@Strain 0.2 %,
Thickness 40.0 - 60.0 mm
Temper T451; Standard EN 485-2
 >= 250 MPa
@Strain 0.2 %,
Thickness 12.5 - 40.0 mm
Temper T451; Standard EN 485-2
 >= 260 MPa
@Strain 0.2 %,
Thickness 7.90 - 12.5 mm
Temper T451; Standard EN 485-2
 265 MPa
@Strain 0.2 %,
Thickness 25.0 - 60.0 mm
Typical Strength; Standard EN 485-2
 265 MPa
@Strain 0.2 %,
Thickness 60.0 - 155 mm
Typical Strength; Standard EN 485-2
 270 MPa
@Strain 0.2 %,
Thickness 7.90 - 25.0 mm
Typical Strength; Standard EN 485-2
 >= 420 MPa
@Strain 0.2 %,
Thickness 80.0 - 115 mm
Temper T451; Standard EN 485-2
Elongation at Break >= 6.0 %
@Thickness 80.0 - 115 mm
Temper T451; Standard EN 485-2
 >= 7.0 %
@Thickness 60.0 - 80.0 mm
Temper T451; Standard EN 485-2
 >= 12 %
@Thickness 12.5 - 40.0 mm
Temper T451; Standard EN 485-2
 >= 12 %
@Thickness 40.0 - 60.0 mm
Temper T451; Standard EN 485-2
 >= 13 %
@Thickness 7.90 - 12.5 mm
Temper T451; Standard EN 485-2
 17 %
@Thickness 60.0 - 155 mm
Typical Elongation
 20 %
@Thickness 7.90 - 25.0 mm
Typical Elongation
 20 %
@Thickness 25.0 - 60.0 mm
Typical Elongation
Modulus of Elasticity 72.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000360 - 0.00000420 ohm-cmTemper T651
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
Thermal Conductivity 125 - 140 W/m-KTemper T651
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 91.4 - 95.5 %as balance
Chromium, Cr <= 0.10 %
Copper, Cu 3.5 - 4.5 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.40 - 1.0 %
Manganese, Mn 0.40 - 1.0 %
Silicon, Si 0.20 - 0.80 %
Zinc, Zn <= 0.25 %
Zr+Ti <= 0.25 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ALIMEX 2017A T451 Aluminum Alloy Rolled
Aluminum 2017-T4; 2017-T451
Alcoa 2324-T39 Aluminum Plate
Alcoa 7055-T7751 Aluminum Plate
Alpase K100-S™ Aluminum Plate

NCONS006 / 160269

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.