Syensqo (Solvay Specialty Polymers) Ixef® 2530/X9027 Polyarylamide, 55% Mineral + Glass Fiber, at Equilibrium (65% RH)
(discontinued **)
Categories:
Polymer
;
Thermoplastic
;
Polyarylamide (PAA)
;
Polyarylamide, Glass Fiber Filled
Material Notes:
The IXEF compounds are a family of semi-crystalline polyarylamide thermoplastics reinforced with glass fibers and/or mineral fillers for injection molding.
Data provided by the manufacturer, Solvay Advanced Polymers.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.85
g/cc
0.0668
lb/in³
dry as molded
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
120
MPa
17400
psi
ASTM D638
Elongation at Break
1.3 %
1.3 %
ASTM D638
Tensile Modulus
18.0
GPa
2610
ksi
ASTM D638
Flexural Yield Strength
175
MPa
25400
psi
ASTM D790
Flexural Modulus
16.5
GPa
2390
ksi
ASTM D790
Izod Impact, Notched
0.500
J/cm
0.937
ft-lb/in
ASTM D256
Izod Impact, Unnotched
2.80
J/cm
5.25
ft-lb/in
ASTM D256
Thermal Properties
Metric
English
Comments
Melting Point
240
°C
464
°F
Processing Properties
Metric
English
Comments
Feed Temperature
250
-
280
°C
482
-
536
°F
Rear Barrel Temperature
250
-
280
°C
482
-
536
°F
Compression Zone
Middle Barrel Temperature
250
-
280
°C
482
-
536
°F
Homogenization Zone
Front Barrel Temperature
260
-
290
°C
500
-
554
°F
Nozzle Zone
Melt Temperature
<=
270
°C
<=
518
°F
Mold Temperature
120
-
140
°C
248
-
284
°F
Needed to develop high crystallinity
Injection Pressure
50.0
-
250
MPa
7250
-
36300
psi
Hold Pressure
30.0
-
150
MPa
4350
-
21800
psi
Back Pressure
0.000
-
1.00
MPa
0.000
-
145
psi
**
Materials flagged as discontinued (
) are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.
Users of our Advanced Search (registration required) may exclude discontinued materials from search results.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Envalior Arnitel® XG5855 TPC-ET, Extrusion Grade
Envalior Arnitel® PM460-H TPC-ET, Injection Molding, Heat Stabilized
Envalior Arnitel® EM740 74 Shore D, Extrusion Grade Copolyester Elastomer (North America)
Envalior Arnitel® EM631-HB TPC-ET
Envalior Arnitel® EB463 TPC-ET, Blow Molding Grade
PSOLO5 / 68343
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.