MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

MRC Polymers NAXELL™ PC210MR General Purpose Polycarbonate, Medium MFR, with Release
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes:
  • Medium melt without impact modification
  • MFR can be modified between 10 to 40 g/10min
  • Can be UV stabilized
  • Internal and external lubricant can be added
  • Generally for black and gray colors only
  • FR package can be added

Information provided by MRC Polymers Inc.

Key Words: PC
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
@Thickness 3.17 mm
0.0050 - 0.0080 in/in
@Thickness 0.125 in
ASTM D955
Melt Flow 12 g/10 min
@Load 1.20 kg,
Temperature 300 °C
12 g/10 min
@Load 2.65 lb,
Temperature 572 °F
nominal; ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 57.9 MPa
@Thickness 3.17 mm,
Temperature 22.8 °C
8400 psi
@Thickness 0.125 in,
Temperature 73.0 °F
ASTM D638
Flexural Strength 96.5 MPa
@Thickness 3.17 mm,
Temperature 22.8 °C
14000 psi
@Thickness 0.125 in,
Temperature 73.0 °F
ASTM D790
Flexural Modulus 2.34 GPa
@Thickness 3.17 mm,
Temperature 22.8 °C
340 ksi
@Thickness 0.125 in,
Temperature 73.0 °F
ASTM D790
Izod Impact, Notched 6.41 J/cm
@Thickness 3.17 mm,
Temperature 22.8 °C
12.0 ft-lb/in
@Thickness 0.125 in,
Temperature 73.0 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 132 °C
@Thickness 3.17 mm
270 °F
@Thickness 0.125 in
un-annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 125 °C
@Thickness 3.17 mm
257 °F
@Thickness 0.125 in
un-annealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 260 - 271 °C500 - 520 °F
Middle Barrel Temperature 266 - 277 °C510 - 530 °F
Front Barrel Temperature 271 - 282 °C520 - 540 °F
Nozzle Temperature 271 - 282 °C520 - 540 °F
Melt Temperature 271 - 293 °C520 - 560 °F
Mold Temperature 48.9 - 76.7 °C120 - 170 °F
Drying Temperature 116 °C240 °F
Dry Time 4 hour4 hour
Moisture Content <= 0.020 %<= 0.020 %
Dew Point <= -17.8 °C<= 0.000 °F
Drying Air Flow Rate 22.7 - 28.3 l/min0.800 - 1.00 ft³/min (CFM)per lb/hour resin processed
Injection Pressure 68.9 - 138 MPa10000 - 20000 psi
Back Pressure 0.345 - 1.21 MPa50.0 - 175 psi
Vent Depth 0.00762 cm0.00300 in
Cushion 0.635 cm0.250 in
Screw Speed 50 - 75 rpm50 - 75 rpm
 
Descriptive Properties
Fill RateModerate
Hold Pressure40-60% of injection pressure
Packing Pressure50-75% of injection pressure

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Trinseo EMERGE™ 8600-10 Polycarbonate

PMRC032 / 89461

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.