MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Lubrizol Estane® ZHF 95AT3 Thermoplastic Polyurethane, Flame Retardant
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyether Grade

Material Notes: Type: Estane® ZHF 95AT3 TPU is a zero halogen flame retardant polyether based thermoplastic polyurethane compound.

Features: Outstanding flame retardant properties, especially suited for tray cables.

Uses: Cable jacket and hose and tube and injection molding and fabric coating

Available in Americas, Europe, Middle East, Africa, India and Asia

Information Provided by The Lubrizol Corporation

Key Words: TPU
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.24 g/ccASTM D792
Maximum Moisture Content 0.020
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 95
@Time 5.00 sec
ASTM D2240
Tensile Strength 1500 psi
@Temperature 121 °C,
Time 605000 sec
Air Oven
 1700 psi
@Temperature 113 °C,
Time 605000 sec
Air Oven
 2000 psi
@Temperature 100 °C,
Time 605000 sec
IRM 902 Oil
Tensile Strength, Ultimate 2000 psiASTM D412
Elongation at Break 360 %ASTM D412
 270 %
@Treatment Temp. 121 °C,
Time 605000 sec
Air Oven
 288 %
@Treatment Temp. 100 °C,
Time 605000 sec
IRM 902 Oil
 324 %
@Treatment Temp. 113 °C,
Time 605000 sec
Air Oven
100% Modulus 0.00960 GPa
@Strain 100 %
ASTM D412
300% Modulus 0.0124 GPa
@Strain 300 %
ASTM D412
Tear Strength 90.0 pliTrouser; ASTM D470
Graves Tear Strength 340 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 300
@Load 1.00 kg
H-18 wheel; ASTM D3389
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 5.60e+12 ohm-cmASTM D257
Surface Resistivity per Square 5.60e+14 ohmASTM D257
Dielectric Constant 4.5
@Frequency 1000 Hz
ASTM D2520
 5.7
@Frequency 1e+6 Hz
ASTM D2520
Dissipation Factor 0.040
@Frequency 1000 Hz
ASTM D2520
 0.050
@Frequency 1e+6 Hz
ASTM D2520
 
Thermal PropertiesOriginal ValueComments
Melting Point 175 °CDSC
Glass Transition Temp, Tg -30.0 °CDSC
Flammability, UL94 V-0
@Thickness 0.762 mm
Vertical Flame Test; ASTM D3801
Oxygen Index 38 %ASTM D2863
 
Processing PropertiesOriginal ValueComments
Zone 1 160 °CExtrusion
Zone 2 165 °CExtrusion
Zone 3 170 °CExtrusion
Zone 4 175 °CExtrusion
Adapter Temperature 180 °C5, Extrusion
Die Temperature 180 °C6, Zone 1, Extrusion
 180 °CZone 2, Extrusion
Drying Temperature 82.0 °C
Dry Time 2.00 - 4.00 hour
Dew Point -40.0 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 95 P 5003 TPU-Polyether
SPS Guang Zhou POFLEX™ EP8300 Cable Grade TPU
AlphaGary Garathane™ X 94-350 B Polyurethane based compound
Lubrizol ESTANE® 58244 Ether Based Thermoplastic Polyurethane
Lubrizol Estane® ZHF 80AT3 Thermoplastic Polyurethane, Flame Retardant

PNOVEON600 / 121491

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.