MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Plastcom SLOVALEN PH 49 GF 30 Polypropylene Homopolymer, 30% Glass Fiber
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 30% Glass Fiber Filler

Material Notes: Features

Modified homopolymer PP for injection moulding, chemically reinforced with 30% glass fiber, contains the modifier of mechanical properties. Increased strength in comparison with unfilled PP. Applied in all industry branches. Increased strength, toughness, tensile modulus due to the modification. Delivered in natural and in the full RAL color scale. Moderately increased toughness and lower MFI in comparison with PH 69 GF 30.

Application: Injection Moulding

Information Provided by Plastcom spol. s r.o.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccSTN 64 0111
Linear Mold Shrinkage 0.0065 cm/cmSTN 64 0808
Linear Mold Shrinkage, Transverse 0.0128 cm/cmSTN 64 0808
Melt Flow 4.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
STN EN ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 100 MPaSTN EN ISO 527-2
Elongation at Break 2.0 %STN EN ISO 527-2
Tensile Modulus 6850 MPaSTN EN ISO 527-2
Flexural Strength 115 MPaSTN EN ISO 178
Flexural Modulus 5500 MPaSTN EN ISO 178
Charpy Impact Unnotched 52.0 kJ/m²
@Temperature -20.0 °C
STN EN ISO 179
 55.0 kJ/m²
@Temperature 23.0 °C
STN EN ISO 179
Charpy Impact, Notched 11.0 kJ/m²
@Temperature -20.0 °C
STN EN ISO 179
 13.0 kJ/m²
@Temperature 23.0 °C
STN EN ISO 179
 
Thermal PropertiesOriginal ValueComments
Melting Point 160 °CDSC; STN EN ISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 160 °CSTN EN ISO 75/A
Vicat Softening Point 155 °CB; STN EN ISO 306
 
Processing PropertiesOriginal ValueComments
Melt Temperature 200 - 250 °C
Mold Temperature 40.0 - 80.0 °C
Injection Pressure 70.0 - 120 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Akro-Plastic Akromid® A3 GF 30 1 L natural (4715) PA66 + PP, Dry, 30% Glass Filled
Asahi Kasei Thermylene® P4-30FG-0522 PP-GF30FR
Envalior TEPEX® dynalite 104-RG600(x)/47% Roving Glass – PP Consolidated Composite Laminate
Plastcom PLASTALEN® PH 69 GF 30 Polypropylene reinforced with glass fiber
Plastcom SLOVALEN PH 49 GF 25 PP, 25% glass fibre, mod. of mech. properties

PPLACO073 / 106951

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.