MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

SABIC LNP™ COLORCOMP™ Compound W1000EXP Polybutylene Terephthalate (PBT) (Americas)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: LNP COLORCOMP W1000EXP compound is based on unfilled Polybutylene Terephthalate (PBT) resin.

Features: Aesthetics and Appearance,Custom Color

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.31 g/cc1.31 g/ccASTM D792
 1.316 g/cc1.316 g/ccASTM D792
Water Absorption 0.080 %
@Time 86400 sec
0.080 %
@Time 24.0 hour
ASTM D570
Moisture Absorption 0.0200 %0.0200 %Injection Molding
Viscosity 600000 cP600000 cPmelt; SABIC method
Linear Mold Shrinkage, Flow  0.0090 - 0.016 cm/cm
@Thickness 0.750 - 2.30 mm
0.0090 - 0.016 in/in
@Thickness 0.0295 - 0.0906 in
SABIC method
 0.015 - 0.023 cm/cm
@Thickness 2.30 - 4.60 mm
0.015 - 0.023 in/in
@Thickness 0.0906 - 0.181 in
SABIC method
Linear Mold Shrinkage, Transverse  0.010 - 0.017 cm/cm
@Thickness 0.750 - 2.30 mm
0.010 - 0.017 in/in
@Thickness 0.0295 - 0.0906 in
SABIC method
 0.016 - 0.024 cm/cm
@Thickness 2.30 - 4.60 mm
0.016 - 0.024 in/in
@Thickness 0.0906 - 0.181 in
SABIC method
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 117117ASTM D785
Tensile Strength at Break 51.0 MPa7400 psi50 mm/min; ASTM D638
Tensile Strength, Yield 51.0 MPa7400 psi50 mm/min; ASTM D638
Elongation at Break 200 %200 %50 mm/min; ASTM D638
Flexural Strength 82.0 MPa11900 psibrk, 1.3 mm/min, 50 mm span; ASTM D790
 82.0 MPa11900 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.34 GPa339 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 53.0 J39.1 ft-lbASTM D256
Izod Impact, Unnotched 16.02 J/cm30.01 ft-lb/inASTM D4812
Gardner Impact 40.0 J29.5 ft-lbASTM D3029
 40.0 J29.5 ft-lbASTM D3029
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 4.00e+16 ohm-cm>= 4.00e+16 ohm-cmASTM D257
Dielectric Constant  3.1
@Frequency 1e+6 Hz
3.1
@Frequency 1e+6 Hz
ASTM D150
 3.3
@Frequency 100 Hz
3.3
@Frequency 100 Hz
ASTM D150
Dielectric Strength  15.7 kV/mm
@Thickness 3.20 mm
399 kV/in
@Thickness 0.126 in
in air; ASTM D149
 15.7 kV/mm
@Thickness 3.20 mm
399 kV/in
@Thickness 0.126 in
in oil; ASTM D149
 23.2 kV/mm
@Thickness 1.60 mm
589 kV/in
@Thickness 0.0630 in
in air; ASTM D149
 23.2 kV/mm
@Thickness 1.60 mm
589 kV/in
@Thickness 0.0630 in
in oil; ASTM D149
Dissipation Factor  0.0020
@Frequency 100 Hz
0.0020
@Frequency 100 Hz
ASTM D150
 0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 180 - 240 sec180 - 240 secASTM D495
Comparative Tracking Index >= 600 V>= 600 VUL 746A
Hot Wire Ignition, HWI  7.0 - 15 sec
@Thickness >=1.50 mm
7.0 - 15 sec
@Thickness >=0.0591 in
UL 746A
 15 - 30 sec
@Thickness >=3.00 mm
15 - 30 sec
@Thickness >=0.118 in
UL 746A
 30 - 60 sec
@Thickness >=6.00 mm
30 - 60 sec
@Thickness >=0.236 in
UL 746A
High Amp Arc Ignition, HAI >= 120 arcs
@Thickness >=1.50 mm
>= 120 arcs
@Thickness >=0.0591 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/min0.394 - 1.00 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  81.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
45.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 139 µm/m-°C
@Temperature 60.0 - 138 °C
77.2 µin/in-°F
@Temperature 140 - 280 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 154 °C
@Thickness 6.40 mm
309 °F
@Thickness 0.252 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 54.0 °C
@Thickness 6.40 mm
129 °F
@Thickness 0.252 in
unannealed; ASTM D648
UL RTI, Electrical 120 °C248 °FUL 746B
UL RTI, Mechanical with Impact 120 °C248 °FUL 746B
UL RTI, Mechanical without Impact 140 °C284 °FUL 746B
Flammability, UL94 HB
@Thickness >=0.840 mm
HB
@Thickness >=0.0331 in
UL 94
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 240 - 255 °C464 - 491 °F
Zone 2 240 - 255 °C464 - 491 °F
Zone 3 245 - 260 °C473 - 500 °F
Melt Temperature 245 - 260 °C473 - 500 °FInjection Molding
Mold Temperature 50.0 - 75.0 °C122 - 167 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 12.0 hour12.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 80 %40 - 80 %
Vent Depth 0.00130 - 0.00250 cm0.000512 - 0.000984 in
Screw Speed 50 - 100 rpm50 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80578 / 288525

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.