MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Park Aerospace Nelcote® V-376 Cyanate Ester Epoxy Prepregs, 4503 Quartz Reinforced
Categories: Polymer; Thermoset; Epoxy

Material Notes: Nelcote® V-376 is a Cyanate Ester matrix providing excellent electrical and mechanical properties for harsh aircraft, shipboard, and undersea applications for Radomes, Antenna, and Reflectors. Simple processing and good handling characteristics make V-376 an ideal alternative to BMI and polyimide resin systems. GC110 LM qualified specifications.

Key Features and Benefits:

  • Cyanate Ester resin provides outstanding electrical properties (Dk, Df)
  • Excellent Moisture resistance properties
  • Simplified handling and processing characteristics
  • Minimal degradation of mechanical properties in Hot/Wet environments
  • Self-Adhesive to many types of foam and honeycomb core

Applications/Qualifications:

  • Radomes
  • Reflectors
  • Antenna
  • Signature Control

Information provided by Park Electrochemical Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Volatiles <= 1.5 %
Water Absorption 0.67 %by weight; 14 day soak at 160°F
Thickness 0.0100 milcured laminate, per ply
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 71000 psi
@Temperature 149 °C
0° Direction, Wet; ASTM D638
 96000 psi
@Temperature 23.9 °C
0° Direction, Dry; ASTM D638
Tensile Modulus 3300 ksi
@Temperature 149 °C
Wet; ASTM D638
 3600 ksi
@Temperature 23.9 °C
Dry; ASTM D638
Flexural Strength 103 ksi
@Temperature 23.9 °C
0° Direction, Dry; ASTM D790
Flexural Modulus 3400 ksi
@Temperature 23.9 °C
0° Direction, Dry; ASTM D790
Compressive Strength 46.0 ksi
@Temperature 149 °C
Wet; ASTM D695
 58.0 ksi
@Temperature 149 °C
Dry; ASTM D695
 69.0 ksi
@Temperature 23.9 °C
Dry; ASTM D695
Compressive Modulus 3600 ksi
@Temperature 23.9 °C
Dry; ASTM D695
 3600 ksi
@Temperature 149 °C
Wet; ASTM D695
 3700 ksi
@Temperature 149 °C
Dry; ASTM D695
Shear Strength 9.20 ksi
@Temperature 23.9 °C
Short Beam; Dry; ASTM D2344
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.3
@Frequency 9.375e+9 Hz
Dissipation Factor 0.0070
@Frequency 9.375e+9 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 28.9 µin/in-°FZ-Axis
Glass Transition Temp, Tg 148 °CDMA; without post-cure
 178 °CDMA; with post-cure
 
Processing PropertiesOriginal ValueComments
Gel Time 3.00 - 30.0 min
@Temperature 135 °C
Shelf Life 12.0 Month
@Temperature -17.8 °C
 
Descriptive Properties
Fabric Area Weight (g/m²)112
Resin Flow (%)13-33325°F, 50psi
Resin Solids Content (%)35-41

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Rogers Corporation RO4350B Glass-Reinforced Hydrocarbon and Ceramic Laminate with Thin Film Resistor Foil

PPARK079 / 89351

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.