MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Dow Dow™ DMDA-8007 NT 7 HDPE
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE)

Material Notes: Product Description: Dow DMDA-8007 NT 7 is a narrow molecular weight distribution high density homopolymer designed to offer excellent stiffness, low warpage, good/acceptable toughness, and good moldability. The resin is ideally suited for injection molded crates, cases, trays, tote bins, and other objects requiring high rigidity. This resin is also suitable for cast film extrusion processing.
  • Excellent stiffness/modulus
  • Excellent warp resistance
  • Molded parts have high gloss, low odor
Complies with: US FDA 21 CFR 177.1520©2.2; Canadian HPFB No Objection; EU, No 10/2011. Consult the regulations for complete details.

Availability: Asia Pacific; Latin America; North America

Additive: Antiblock: No; Processing Aid: No; Slip: No

Agency Ratings: EU No 10/2011; FDA 21 CFR 177.1520© 2.2; HPFB (Canada) No Objection

Form: Pellets

Processing Method: Cast Film; Injection Molding

Information provided by The Dow Chemical Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.967 g/ccASTM D792
ESCR 100% Igepal® 2.0 hour
@Temperature 50.0 °C
F50; ASTM D1693
Melt Flow 8.3 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 180 g/10 min
@Load 21.6 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 2600 psiMolded and tested in accordance with ASTM D4976; ASTM D638
Film Tensile Strength at Yield, MD 2950 psi
@Thickness 0.0254 mm
Cast Film; ASTM D882
Film Tensile Strength at Yield, TD 3240 psi
@Thickness 0.0254 mm
Cast Film; ASTM D882
Tensile Strength, Yield 4500 psiMolded and tested in accordance with ASTM D4976; ASTM D638
Film Elongation at Break, MD 670 %
@Thickness 0.0254 mm
Cast Film; ASTM D882
Film Elongation at Break, TD 490 %
@Thickness 0.0254 mm
Cast Film; ASTM D882
Elongation at Break 350 %Molded and tested in accordance with ASTM D4976; ASTM D638
Elongation at Yield 6.0 %Molded and tested in accordance with ASTM D4976; ASTM D638
Flexural Modulus 205000 psi2% Secant, Molded and tested in accordance with ASTM D4976; ASTM D790B
2% Secant Modulus 116000 psi
@Thickness 0.0254 mm
MD, Cast Film; ASTM D882
 136000 psi
@Thickness 0.0254 mm
TD, Cast Film; ASTM D882
Tensile Impact Strength 80.0 ft-lb/in²Type S; ASTM D1822
Elmendorf Tear Strength MD 36 g
@Thickness 0.0254 mm
Cast Film; ASTM D1922
Elmendorf Tear Strength TD 160 g
@Thickness 0.0254 mm
Cast Film; ASTM D1922
Dart Drop Test 24.0 g
@Thickness 0.0254 mm
Cast Film; ASTM D1709A
 
Thermal PropertiesOriginal ValueComments
Melting Point 271 °F
Crystallization Temperature 248 °F
Vicat Softening Point 268 °FASTM D1525
Brittleness Temperature <= -105 °FASTM D746
 
Optical PropertiesOriginal ValueComments
Haze 8.0 %
@Thickness 0.0254 mm
Cast Film; ASTM D1003
Gloss 75 %
@Thickness 0.0254 mm
45°, Cast Film; ASTM D2457
 
Processing PropertiesOriginal ValueComments
Melt Temperature 500 °FExtrusion
 
Descriptive Properties
Film Puncture Resistance7 ft-lb/in31.0 mil

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDOWF442 / 311135

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.