MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Eastman Cadence™ GS1 Copolyester for film calendering  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyester Film

Material Notes: Eastman Cadence™ GS1 is Eastman's original copolyester for film calendering. Calendered films made of Eastman Cadence™ copolyesters are non-crystallizing, are halogen-free, offer wide calendering and thermoforming windows and have good low-temperature toughness. They are cooperative in secondary operations such as solvent-bonding, lamination, decoration, coldforming, punching/cutting and embossment. Eastman Cadence™ resins require no pre-drying or additional stabilizers. This product has been GREENGUARD INDOOR AIR QUALITY CERTIFIED® Eastman Cadence GS5 is an amorphous copolyester with improved processability for film calendering. Calendered films made of Eastman Cadence copolyesters are non-crystallizing, are halogen-free, offer wide calendering and thermoforming windows and have good low-temperature toughness. They are cooperative in secondary operations such as solvent-bonding, lamination, decoration, cold-forming, punching/cutting and embossment.

Eastman Cadence resins require no pre-drying or additional stabilizers.

Application/Uses

  • Appliance films
  • Architectural laminates
  • Automotive films
  • Bags
  • Decorative laminates
  • Electronic laminates
  • Floor coverings
  • Furniture/Furniture trim
  • Labels
  • Outdoor films
  • Packaging
  • Printable films
  • Shrink film
  • Transaction cards
  • Transportation laminates
  • Wall coverings

Reported typical properties are preliminary. Information was provided by Eastman.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.28 g/cc0.0462 lb/in³ASTM D1505
Water Absorption 0.16 %
@Time 86400 sec
0.16 %
@Time 24.0 hour
Immersion; ASTM D570
Water Vapor Transmission 7.00 g/m²/day0.451 g/100 in²/dayASTM F372
Oxygen Transmission 7.00 cc-mm/m²-24hr-atm17.8 cc-mil/100 in²-24hr-atmASTM D3985
Viscosity Measurement 0.710.71Inherent Viscosity; EMN-A-AC-G-V-1
Thickness 170 microns6.69 milThickness of film tested; ASTM D374
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 49.0 MPa7110 psiASTM D882
Film Tensile Strength at Yield, TD 49.0 MPa7110 psiASTM D882
Film Elongation at Break, MD 420 %420 %ASTM D882
Film Elongation at Break, TD 300 %300 %ASTM D882
Film Elongation at Yield, MD 5.0 %5.0 %ASTM D882
Film Elongation at Yield, TD 5.0 %5.0 %ASTM D882
Secant Modulus, MD 1.60 GPa232 ksiASTM D882
Secant Modulus, TD 1.60 GPa232 ksiASTM D882
Puncture Energy  0.700 J
@Temperature -20.0 °C
0.516 ft-lb
@Temperature -4.00 °F
Energy @ Max. Load; ASTM D3763
 1.20 J
@Temperature 0.000 °C
0.885 ft-lb
@Temperature 32.0 °F
Energy @ Max. Load; ASTM D3763
 1.60 J
@Temperature 23.0 °C
1.18 ft-lb
@Temperature 73.4 °F
Energy @ Max. Load; ASTM D3763
Elmendorf Tear Strength MD 724 g724 gASTM D1922
Elmendorf Tear Strength TD 897 g897 gASTM D1922
Elmendorf Tear Strength, MD 4.30 g/micron109 g/milASTM D1922
Elmendorf Tear Strength, TD 5.30 g/micron135 g/milASTM D1922
Film Tensile Strength at Break, MD 63.0 MPa9140 psiASTM D882
Film Tensile Strength at Break, TD 46.0 MPa6670 psiASTM D882
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 3.87e+16 ohm-cm3.87e+16 ohm-cmASTM D257
Surface Resistivity per Square 1.19e+16 ohm1.19e+16 ohmASTM D257
Dielectric Constant  2.68
@Frequency 1e+6 Hz
2.68
@Frequency 1e+6 Hz
ASTM D150
 2.88
@Frequency 1000 Hz
2.88
@Frequency 1000 Hz
ASTM D150
Dielectric Strength 14.6 kV/mm371 kV/inShort time, 500 V/sec rate-of-rise; ASTM D149
Dissipation Factor  0.021
@Frequency 1e+6 Hz
0.021
@Frequency 1e+6 Hz
ASTM D150
 0.022
@Frequency 1000 Hz
0.022
@Frequency 1000 Hz
ASTM D150
Arc Resistance 131 sec131 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear 76.6 µm/m-°C
@Temperature -30.0 - 30.0 °C
42.6 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
Specific Heat Capacity  1.30 J/g-°C
@Temperature 60.0 °C
0.310 BTU/lb-°F
@Temperature 140 °F
DSC
 1.72 J/g-°C
@Temperature 100 °C
0.410 BTU/lb-°F
@Temperature 212 °F
DSC
 1.84 J/g-°C
@Temperature 150 °C
0.440 BTU/lb-°F
@Temperature 302 °F
DSC
 1.97 J/g-°C
@Temperature 200 °C
0.470 BTU/lb-°F
@Temperature 392 °F
DSC
 2.05 J/g-°C
@Temperature 250 °C
0.490 BTU/lb-°F
@Temperature 482 °F
DSC
Deflection Temperature at 0.46 MPa (66 psi) 70.0 °C158 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 62.0 °C144 °FASTM D648
Vicat Softening Point 81.0 °C178 °FASTM D1525
Glass Transition Temp, Tg 81.0 °C178 °FDSC
Oxygen Index 23.5 %23.5 %ASTM D2863
 
Optical PropertiesMetricEnglishComments
Haze 2.7 %2.7 %ASTM D1003
Gloss 107 %107 %@ 60°; ASTM D2457
Transmission, Visible 90 %90 %ASTM D1003 modified
 
Descriptive Properties
Greenguard Indoor Air Quality Certifiedyes

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Teijin Films Mylar® LBT-2 Polyester Packaging Film, 48 Gauge
DuPont Teijin Films Mylar® RL4 Polyester Packaging Film, 50 Gauge
DuPont Teijin Films Mylar® RL42 Polyester Packaging Film, 50 Gauge
Eastman Cadence™ GS2 Copolyester for film calendering
DuPont Teijin Films Mylar® OB12AF Polyester Packaging Film, 50 Gauge

PE8901 / 109243

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.