MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 4155 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 4100 series are engineered materials designed primarily for demanding automotive and industrial applications. Available in both black and natural, this product is a low density, medium hardness thermoplastic vulcanizate that exhibits excellent compression set, flex fatigue, high and low temperature performance. The material can be processed by injection molding, blow molding and extrusion for applications such as seals, gaskets, chemical resistant hose and tube, boots and bellows.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Excellent Elastic Recovery; Fatigue Resistant; Good Adhesion; Good Flexibility; Good Melt Strength; Good Moldability; Good Processability; Good Surface Finish; High Melt Stability; Low Density; Low Specific Gravity; Low Temperature Flexibility; Medium Hardness; Medium Heat Resistant; Resilient

Uses: Agricultural Applications: Appliance Components; Automotive Applications; Automotive Interior Parts; Automotive Under the Hood; Blow Molding Applications; Grommets; Hose; Industrial Applications; Pipe Seals; Profiles; Rubber Replacement; Seals; White Goods & Small Appliance

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER MS-AR-100 AGN Color: Black; CHRYSLER MS-AR-100 AGN Color: Natural; FORD WSD-M2D378-A1 Color: Black; FORD WSD-M2D378-A1 Color: Natural; GM GMP.E/P.001 Color: Black; GM GMP.E/P.001 Color: Natural; GM GMW/15813 Type 4 Color: Black; GM GMW/15813 Type 4 Color: Natural; GM QK 3531 Type 3 Color: Black; GM QK 3531 Type 3 Color: Natural; HONDA Unspecified Color: Black; RENAULT F.R.M. 7A-10-A11 Color: Black; VAG VW/501 23 Color: Black

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.960 g/cc0.0347 lb/in³ISO 1183
Viscosity 320 cP
@Shear Rate 206 1/s,
Temperature 200 °C
320 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  53
@Time 5.00 sec
53
@Time 0.00139 hour
Extruded; ISO 868
 56
@Time 5.00 sec
56
@Time 0.00139 hour
Injection Molded; ISO 868
Tensile Strength at Break 4.30 MPa624 psiFlow; ISO 37
 5.20 MPa754 psiAcross Flow; ISO 37
 4.73 MPa
@Treatment Temp. 150 °C,
Time 605000 sec
686 psi
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 4.94 MPa
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
716 psi
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain  2.00 MPa
@Strain 100 %
290 psi
@Strain 100 %
Across Flow; ISO 37
 3.10 MPa
@Strain 100 %
450 psi
@Strain 100 %
Flow; ISO 37
 1.60 MPa
@Strain 100 %,
Treatment Temp. 150 °C
232 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
 2.40 MPa
@Strain 100 %,
Treatment Temp. 135 °C
348 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
Elongation at Break 240 %240 %Flow; ISO 37
 550 %550 %Across Flow; ISO 37
 517 %
@Treatment Temp. 150 °C,
Time 605000 sec
517 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 556 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
556 %
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
Tear Strength 22.8 kN/m130 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  14 %
@Temperature 22.8 °C,
Time 79200 sec
14 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 26 %
@Temperature 70.0 °C,
Time 79200 sec
26 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 37 %
@Temperature 125 °C,
Time 252000 sec
37 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
Flammability, UL94  HB
@Thickness 0.610 mm
HB
@Thickness 0.0240 in
BK
 HB
@Thickness 1.52 mm
HB
@Thickness 0.0600 in
NC
 
Processing PropertiesMetricEnglishComments
Processing Temperature 187 - 220 °C369 - 428 °FInjection
Rear Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Middle Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Front Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Nozzle Temperature 187 - 220 °C369 - 428 °FInjection
Zone 1 180 - 200 °C356 - 392 °FExtrusion
Zone 2 180 - 205 °C356 - 401 °FExtrusion
Zone 3 187 - 210 °C369 - 410 °FExtrusion
Zone 4 187 - 210 °C369 - 410 °FExtrusion
Die Temperature 195 - 215 °C383 - 419 °FExtrusion
Melt Temperature 195 - 215 °C383 - 419 °FExtrusion
Mold Temperature 10.0 - 55.0 °C50.0 - 131 °FInjection
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Screw Speed 100 - 200 rpm100 - 200 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPV 4139D Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 6775N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 6765N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 4175 Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 4165 Thermoplastic Vulcanizate

PTEKNQ1156 / 237647

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.