MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Geon® Performance Solutions Vinyl Flexible A7509  (discontinued **)
Categories: Polymer; Thermoplastic; Vinyl (PVC); PVC, Flexible Grade; PVC, Transparent

Material Notes:

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.021 - 0.025 cm/cm0.021 - 0.025 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7575ASTM D2240
 67
@Time 15.0 sec
67
@Time 0.00417 hour
ASTM D2240
Tensile Strength at Break 13.8 MPa2000 psi510 mm/min; ASTM D638
Tensile Stress at Strain 6.55 MPa
@Strain 100 %
950 psi
@Strain 100 %
510 mm/min; ASTM D638
Elongation at Break 420 %420 %510 mm/min; ASTM D638
Tear Strength 45.5 kN/m260 pliDie C, 510 mm/min; ASTM D624
Clash Berg Modulus  0.310 GPa
@Temperature -37.0 °C
45.0 ksi
@Temperature -34.6 °F
ASTM D1043
 0.323 GPa
@Temperature 23.0 °C
46.8 ksi
@Temperature 73.4 °F
ASTM D1043
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -40.0 °C-40.0 °FASTM D746
 
Processing PropertiesMetricEnglishComments
Melt Temperature 174 - 179 °C345 - 354 °F
 188 - 199 °C370 - 390 °F
 
Compliance PropertiesMetricEnglishComments
FDA YesYesUnspecified Rating
USP Class VI YesYes
 
Descriptive Properties
AppearanceClear/Transparent
FeaturesHigh Gloss
FormsPellets
Processing MethodExtrusion
 Injection Molding
Regional AvailabilityAfrica & Middle East
 Asia Pacific
 Europe
 North America
 South America
UsesMedical Appliances
 Medical/Healthcare Applications

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PH1PN8361 / 102197

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.