MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Versalis Flexirene® CM 50 Butene Copolymer Linear Low Density Polyethylene
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Butene, Film

Material Notes: Flexirene CM 50 is a butene copolymer with medium density (C4-LLDPE), with antioxidants, suitable for cast film extrusion.

Main Applications: Flexirene CM 50 is a highly stiff product and it is recommended for the production of coextruded stretch film in slip-cling formulations where it acts as the slip layer.

Information provided by Polimeri Europa.

Versalis is the Eni subsidiary containing the plastics and rubber businesses.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.938 g/cc0.938 g/ccISO 1183
Thickness 10.0 - 50.0 microns0.394 - 1.97 milRecommended
Melt Flow 4.1 g/10 min
@Load 2.16 kg,
Temperature 190 °C
4.1 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 17.0 MPa2470 psiISO 527-3
Film Tensile Strength at Yield, TD 16.0 MPa2320 psiISO 527-3
Film Elongation at Break, MD 600 %600 %ISO 527-3
Film Elongation at Break, TD 700 %700 %ISO 527-3
Coefficient of Friction, Dynamic >= 0.50>= 0.50ISO 8295
Elmendorf Tear Strength, MD 0.8152 g/micron20.71 g/milISO 6383-2
Elmendorf Tear Strength, TD 2.038 g/micron51.77 g/milISO 6383-2
Dart Drop Test 45.0 g0.0992 lbF50; ISO 7765-1
Film Tensile Strength at Break, MD 25.0 MPa3630 psiISO 527-3
Film Tensile Strength at Break, TD 20.0 MPa2900 psiISO 527-3
1% Secant Modulus, MD 350 MPa50800 psiISO 527-3
1% Secant Modulus, TD 370 MPa53700 psiISO 527-3
 
Thermal PropertiesMetricEnglishComments
Melting Point 127 °C261 °FInternal method
Vicat Softening Point 118 °C
@Load 1.00 kg
244 °F
@Load 2.20 lb
ISO 306/A
Brittleness Temperature <= -70.0 °C<= -94.0 °FASTM D746
 
Optical PropertiesMetricEnglishComments
Haze 8.0 %8.0 %ISO 14782
Gloss 75 %75 %45°; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil PP1013H1 Polypropylene Homopolymer
Celanese Hostaform® MT24U01 POM, Medical Technology
Versalis Riblene® MP 31 Low Density Polyethylene - Injection Molding
Versalis Flexirene® MR 50 A Linear Low Density Polyethylene
LyondellBasell Purell PE GF 4750 High Density Polyethylene (HDPE), Blow Molding Grade

PENG098 / 124492

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.