MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LG Chemical NBR 3280 High Acrylonitrile Polymer
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Description: NBR 3280 is a copolymer of butadiene and acrylonitrile manufactured by cold emulsion polymerization technology of Goodyear Tire and Rubber Company, USA. NBR 3280 is a non staining, high mooney viscosity, and high acrylonitrile polymer designed to aid in processing operations such as calendaring and extruding for oil and fuel service products. NBR 3280 offers high resistance to fuels, solvents, oils and gas permeation, and also it can be used for economic compound by high loading of plasticizer on compound recipe.

Applications: NBR 3280 is recommended to use in industrial and automotive parts such as fuel hoses and packings.

CAS No: 9003-18-3

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.990 g/cc0.990 g/cc
Volatiles 0.30 %0.30 %
Mooney Viscosity 80.5
@Temperature 100 °C
80.5
@Temperature 212 °F
ML 1+4
Ash <= 0.50 %<= 0.50 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  52
@Treatment Temp. 25.0 °C,
Time 259000 sec
52
@Treatment Temp. 77.0 °F,
Time 72.0 hour
Aged fuel C
 73
@Treatment Temp. 145 °C,
Time 1190 sec
73
@Treatment Temp. 293 °F,
Time 0.330 hour
Cured
 74
@Treatment Temp. 100 °C,
Time 259000 sec
74
@Treatment Temp. 212 °F,
Time 72.0 hour
Aged ASTM D #3 Oil
 76
@Treatment Temp. 100 °C,
Time 259000 sec
76
@Treatment Temp. 212 °F,
Time 72.0 hour
Circulating Oven Aging
 76
@Treatment Temp. 100 °C,
Time 259000 sec
76
@Treatment Temp. 212 °F,
Time 72.0 hour
Aged ASTM D #1 Oil
Tensile Strength at Break  18.0 MPa
@Treatment Temp. 25.0 °C,
Time 259000 sec
2610 psi
@Treatment Temp. 77.0 °F,
Time 72.0 hour
Aged fuel C
 22.3 MPa
@Treatment Temp. 100 °C,
Time 259000 sec
3230 psi
@Treatment Temp. 212 °F,
Time 72.0 hour
Aged ASTM D #1 Oil
 22.3 MPa
@Treatment Temp. 145 °C,
Time 1190 sec
3230 psi
@Treatment Temp. 293 °F,
Time 0.330 hour
Cured
 22.4 MPa
@Treatment Temp. 100 °C,
Time 259000 sec
3250 psi
@Treatment Temp. 212 °F,
Time 72.0 hour
Aged ASTM D #3 Oil
 22.5 MPa
@Treatment Temp. 100 °C,
Time 259000 sec
3260 psi
@Treatment Temp. 212 °F,
Time 72.0 hour
Circulating Oven Aging
 33.7 MPa
@Treatment Temp. 145 °C,
Time 2990 sec
4890 psi
@Treatment Temp. 293 °F,
Time 0.830 hour
cured; ASTM D412
Elongation at Break  373.2 %
@Treatment Temp. 25.0 °C,
Time 259000 sec
373.2 %
@Treatment Temp. 77.0 °F,
Time 72.0 hour
Aged fuel C
 389.3 %
@Treatment Temp. 100 °C,
Time 259000 sec
389.3 %
@Treatment Temp. 212 °F,
Time 72.0 hour
Aged ASTM D #1 Oil
 391.9 %
@Treatment Temp. 100 °C,
Time 259000 sec
391.9 %
@Treatment Temp. 212 °F,
Time 72.0 hour
Aged ASTM D #3 Oil
 392.6 %
@Treatment Temp. 100 °C,
Time 259000 sec
392.6 %
@Treatment Temp. 212 °F,
Time 72.0 hour
Circulating Oven Aging
 420 %
@Treatment Temp. 145 °C,
Time 1190 sec
420 %
@Treatment Temp. 293 °F,
Time 0.330 hour
Cured
 532 %
@Treatment Temp. 145 °C,
Time 2990 sec
532 %
@Treatment Temp. 293 °F,
Time 0.830 hour
cured; ASTM D412
300% Modulus 17.5 MPa
@Treatment Temp. 145 °C,
Time 2990 sec
2530 psi
@Treatment Temp. 293 °F,
Time 0.830 hour
cured; ASTM D412
Rebound 41.1 %
@Temperature 30.0 °C
41.1 %
@Temperature 86.0 °F
Abrasion 0.27670.2767AKRON
Compression Set 17.4 %
@Temperature 100 °C,
Time 259000 sec
17.4 %
@Temperature 212 °F,
Time 72.0 hour
160°C x 30 min. Cured)
 
Descriptive Properties
Bound AN Content (%)41.5
ColorTan
ComponentsHAF (IRB#7)40 phr, ASTM D3187
 NBR 3280100 phr, ASTM D3187
 Stearic Acid1 phr, ASTM D3187
 Sulfur1.5 phr, ASTM D3187
 TBBS0.7 phr, ASTM D3187
 ZnO3 phr, ASTM D3187
Compound RecipeAntioxidant(3-C)1 phr
 Antioxidant(RD)2 phr
 Carbon Black(SRF)80 phr
 CZ2 phr
 NBR 3280100 phr
 Plasticizer(DOP)10 phr
 Stearic Acid1 phr
 Sulfur0.5 phr
 TT1 phr
 Zinc Oxide5 phr
Rheometer0.6 mints1, 160°C x 12 min, 1° Arc, MDR
 1.2 mint'50, 160°C x 12 min, 1° Arc, MDR
 2.3 mint'90, 160°C x 12 min, 1° Arc, MDR
 27.7 lb-inMH, 160°C x 12 min, 1° Arc, MDR
 3.1 lb-inML, 160°C x 12 min, 1° Arc, MDR
Volume Swell (%)31.2Aged fuel C (23°C x 72hrs)
 -4.9Aged ASTM D #3 Oil (100°C x 72hrs)
 -8.3Aged ASTM D #1 Oil (100°C x 72hrs)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical NBR 6840 High Acrylonitrile Polymer
LG Chemical NBR 6230 High Acrylonitrile Polymer
LG Chemical NBR 6280 High Acrylonitrile Polymer
LG Chemical NBR 3250 High Acrylonitrile Polymer
Lanxess Keltan® 3250 EPDM Rubber

PLAY730 / 148740

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.