MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
A. Schulman Premi-Glas® 1201-15 Polyester SMC
Categories: Polymer; Thermoset; Composite SMC; Polyester, TS; Thermoset Polyester Glass SMC

Material Notes: Premi-Glas® 1201-15 is a 15% glass reinforced thermoset Sheet Molding Compound designed for sinks, shower stall bases and wall applications. Key features and benefits are:
  • Supports ANSI 124.2 and CSA B45.5 requirements for flame, smoke and stain resistance.
  • Available in glass contents ranging from 10% - 20%; standard product has 15% reinforcement.
  • High gloss, non-rippling surface appearance on large flat surfaces and deep draw side walls.
  • Excellent as-molded dimensional tolerances.
  • Outstanding moldability and flow in compression process.
  • Standard color is white.
  • Passes ANSI 124.2/ CSA B,45.5 stain resistance

Data provided by Premix.

A. Schulman has acquired this former Premix product line.

Key Words: Sheet Molding Compound
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.76 g/cc
Linear Mold Shrinkage 0.0020 cm/cmPolymerization Shrinkage
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 35.0 MPaASTM D638
Tensile Modulus 9.00 GPaASTM D638
Flexural Strength 90.0 MPaASTM D790
Flexural Modulus 9.00 GPaASTM D790
Poissons Ratio 0.30
Shear Modulus 3.50 GPaCalculated
Izod Impact, Notched 370 J/mASTM D256
Izod Impact, Unnotched 4.25 J/cmASTM D4812
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 35.0 µm/m-°CZ Direction
CTE, linear, Transverse to Flow 25.0 µm/m-°CXY Direction
Thermal Conductivity 0.300 W/m-K
 
Processing PropertiesOriginal ValueComments
Processing Temperature 150 °CCompression Molding
Clamp Pressure 500 - 1000 psiMolding Pressure
 
Descriptive Properties
Flame Resistancepass at 3 mmANSI Z124.2
Stain ResistancepassANSI Z124.2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
A. Schulman Premi-Glas® 1200-30 Polyester SMC
A. Schulman Premi-Glas® 1200H-20 Polyester SMC
A. Schulman Premi-Glas® 1200H-15 Polyester SMC
A. Schulman Premi-Glas® 2200-15 CR-SX Fiberglass Reinforced SMC
Menzolit Menzolit® SMC 0180 Unsaturated Polyester UP

PPREMIX16 / 58177

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.