MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Haynes 625 alloy, 50% cold reduction
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Excellent strength up to 816°C, good oxidation resistance and aqueous corrosion, excellent forming and welding characteristics. Applications include a variety of high-temperature aerospace, chemical process industry and power industry uses. Widely used in sea water and power plant scrubber applications.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: ASTM B444, ASTM B446, ASTM B704, ASTM B705, ASTM B366, AWS A5.14, UNS N06625, AMS 5599, AMS 5666, AMS 5837, ASTM B443
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.44 g/ccat RT
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 422Converted from Rockwell C hardness.
Hardness, Knoop 464Converted from Rockwell C hardness.
Hardness, Rockwell C 45
Hardness, Vickers 446Converted from Rockwell C hardness.
Tensile Strength, Ultimate 1540 MPa
Tensile Strength, Yield 1270 MPa
@Strain 0.2 %
Elongation at Break 5.0 %in 50.8 mm
Modulus of Elasticity 208 GPaRT
 126 GPa
@Temperature 1000 °C
 142 GPa
@Temperature 900 °C
 153 GPa
@Temperature 800 °C
 163 GPa
@Temperature 700 °C
 171 GPa
@Temperature 600 °C
 179 GPa
@Temperature 500 °C
 186 GPa
@Temperature 400 °C
 192 GPa
@Temperature 300 °C
 199 GPa
@Temperature 200 °C
 201 GPa
@Temperature 100 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000129 ohm-cmRT
 0.000132 ohm-cm
@Temperature 100 °C
 0.000134 ohm-cm
@Temperature 200 °C
 0.000135 ohm-cm
@Temperature 300 °C
 0.000135 ohm-cm
@Temperature 1000 °C
 0.000136 ohm-cm
@Temperature 900 °C
 0.000136 ohm-cm
@Temperature 400 °C
 0.000137 ohm-cm
@Temperature 500 °C
 0.000137 ohm-cm
@Temperature 800 °C
 0.000138 ohm-cm
@Temperature 600 °C
 0.000138 ohm-cm
@Temperature 700 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.8 µm/m-°C
@Temperature 25.0 - 100 °C
 13.1 µm/m-°C
@Temperature 25.0 - 200 °C
 13.4 µm/m-°C
@Temperature 25.0 - 300 °C
 13.8 µm/m-°C
@Temperature 25.0 - 400 °C
 14.2 µm/m-°C
@Temperature 25.0 - 500 °C
 14.8 µm/m-°C
@Temperature 25.0 - 600 °C
 15.4 µm/m-°C
@Temperature 25.0 - 700 °C
 16.0 µm/m-°C
@Temperature 25.0 - 800 °C
 16.7 µm/m-°C
@Temperature 25.0 - 900 °C
 17.4 µm/m-°C
@Temperature 25.0 - 1000 °C
Specific Heat Capacity 0.410 J/g-°CRT
 0.428 J/g-°C
@Temperature 100 °C
 0.455 J/g-°C
@Temperature 200 °C
 0.477 J/g-°C
@Temperature 300 °C
 0.503 J/g-°C
@Temperature 400 °C
 0.527 J/g-°C
@Temperature 500 °C
 0.552 J/g-°C
@Temperature 600 °C
 0.576 J/g-°C
@Temperature 700 °C
 0.600 J/g-°C
@Temperature 800 °C
 0.625 J/g-°C
@Temperature 900 °C
 0.648 J/g-°C
@Temperature 1000 °C
Thermal Conductivity 9.80 W/m-KRT
 10.9 W/m-K
@Temperature 100 °C
 12.5 W/m-K
@Temperature 200 °C
 13.9 W/m-K
@Temperature 300 °C
 15.3 W/m-K
@Temperature 400 °C
 16.9 W/m-K
@Temperature 500 °C
 18.3 W/m-K
@Temperature 600 °C
 19.8 W/m-K
@Temperature 700 °C
 21.5 W/m-K
@Temperature 800 °C
 23.4 W/m-K
@Temperature 900 °C
 25.6 W/m-K
@Temperature 1000 °C
Melting Point 1290 - 1350 °C
Solidus 1290 °C
Liquidus 1350 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al <= 0.40 %
Carbon, C <= 0.10 %
Chromium, Cr 21 %
Cobalt, Co <= 1.0 %
Iron, Fe <= 5.0 %
Manganese, Mn <= 0.50 %
Molybdenum, Mo 9.0 %
Nickel, Ni 62 %As Remainder
Niobium, Nb (Columbium, Cb) 3.7 %Includes Ta
Silicon, Si <= 0.50 %
Titanium, Ti <= 0.40 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Haynes 718 alloy, cold rolled, solution-treated and aged sheet
660 Stainless Steel (A286) cold drawn wire diameter of 2.84 mm, aged at 650°C (1200°F)
Haynes 625 alloy, 10% cold reduction
Haynes 625 alloy, 50% cold reduction, 1065°C anneal for 5 minutes
HP Alloys Alloy 718, 50% Cold Worked

NH62BA / 16742

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.