MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Toyobo Zenite® SEA 30 N LCP, 40% Mineral Fiber Reinforced
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), Mineral Filled

Material Notes: Product Description: Zenite SEA 30 B is a 40% mineral filled grade. This grade offers excellent surface appearance, low warpage, and excellent dimensional stability. Application for this grade is compact camera module, and other thin, small electronic parts.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Filler/Reinforcement: Mineral

Features: Low Warpage

Form: Pellets

Processing Method: Injection Molding

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.85 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0030 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 14500 psiISO 527-2/5
Elongation at Break 4.6 %ISO 527-2/5
Tensile Modulus 1.02e+6 psiISO 527-1
Flexural Strength 14500 psiISO 178
Flexural Modulus 1.02e+6 psiISO 178
Charpy Impact, Notched 3.30 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.50e+16 ohm-cmIEC 62631-3-1
Surface Resistance 3.80e+14 ohmIEC 62631-3-2
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 11.0 µin/in-°FISO 11359-2
 10.0 µin/in-°F
@Temperature 20.0 - 110 °C
below Tg; ISO 11359-2
 10.0 µin/in-°F
@Temperature 110 - 180 °C
above Tg; ISO 11359-2
CTE, linear, Transverse to Flow 52.0 µin/in-°FISO 11359-2
 49.0 µin/in-°F
@Temperature 20.0 - 110 °C
below Tg; ISO 11359-2
 56.0 µin/in-°F
@Temperature 110 - 180 °C
above Tg; ISO 11359-2
Specific Heat Capacity 0.000265 BTU/lb-°FISO 22007-4
Thermal Conductivity 3.30 BTU-in/hr-ft²-°FThruplane; ISO 22007-4
 4.40 BTU-in/hr-ft²-°FCrossflow; ISO 22007-4
 10.0 BTU-in/hr-ft²-°FFlow; ISO 22007-4
Melting Point 626 °FISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 504 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 428 °FUnannealed; ISO 75-2/A
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 554 - 572 °F
Middle Barrel Temperature 572 - 590 °F
Front Barrel Temperature 617 - 644 °F
Nozzle Temperature 635 - 653 °F
Zone 4 626 - 644 °FInjection
Melt Temperature 635 - 653 °F
Mold Temperature 212 - 284 °F
Drying Temperature 302 °F
Dry Time 6.00 hour
Injection Pressure 7250 - 21800 psi
 
Descriptive Properties
Thermal DiffusivityCrossflow, ISO 22007-4
 Flow, ISO 22007-4
 Thruplane, ISO 22007-4

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHCQ6333 / 311026

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.