MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Total MDPE HR 515 Medium Density Polyethylene, Blown Film
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Medium Density (MDPE); Medium Density Polyethylene (MDPE), Film Grade

Material Notes: MDPE HR 515 is a medium density polyethylene produced with hexene as a co-monomer. It shows a broad molecular weight distribution ensuring outstanding processability.

MDPE HR 515 is especially dedicated to high rigidity film applications, particularly in blend and/or coextrusion with LDPE and/or LLDPE.

MDPE HR 515 is suited for many applications, in the field of consumer, food or hygiene packaging.

Information provided by Total Petrochemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.942 g/ccISO 1183
Melt Flow 0.22 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 17.5 g/10 min
@Load 21.6 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 22.0 MPa
@Thickness 0.0400 mm
ISO 527-3
 23.0 MPa
@Thickness 0.0200 mm
ISO 527-3
Film Tensile Strength at Yield, TD 22.0 MPa
@Thickness 0.0400 mm
ISO 527-3
 24.0 MPa
@Thickness 0.0200 mm
ISO 527-3
Film Elongation at Break, MD 450 %
@Thickness 0.0200 mm
ISO 527-3
 580 %
@Thickness 0.0400 mm
ISO 527-3
Film Elongation at Break, TD 540 %
@Thickness 0.0200 mm
ISO 527-3
 660 %
@Thickness 0.0400 mm
ISO 527-3
Flexural Modulus 810 MPa
@Strain <=0.25 %
ISO 178
Elmendorf Tear Strength, MD 0.800 g/micron
@Thickness 0.0200 mm
ISO 6383-2
 1.20 g/micron
@Thickness 0.0400 mm
ISO 6383-2
Elmendorf Tear Strength, TD 13.3 g/micron
@Thickness 0.0200 mm
ISO 6383-2
 15.3 g/micron
@Thickness 0.0400 mm
ISO 6383-2
Dart Drop Test 145 g
@Thickness 0.0200 mm
ISO 7765-1
 190 g
@Thickness 0.0400 mm
ISO 7765-1
Film Tensile Strength at Break, MD 55.0 MPa
@Thickness 0.0400 mm
ISO 527-3
 65.0 MPa
@Thickness 0.0200 mm
ISO 527-3
Film Tensile Strength at Break, TD 51.0 MPa
@Thickness 0.0400 mm
ISO 527-3
 53.0 MPa
@Thickness 0.0200 mm
ISO 527-3
 
Thermal PropertiesOriginal ValueComments
Melting Point 127 °CISO 11357
Vicat Softening Point 124 °CISO 306
 
Processing PropertiesOriginal ValueComments
Processing Temperature 190 - 220 °CExtrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Total MDPE 3802 Blue Medium Density Polyethylene, Stripes
Total MDPE 3802 B Medium Density Polyethylene, Pipes & Fittings
Baystar™ HL 323 MDPE Medium Density Polyethylene, Film Resin
Total MDPE LF 38 YS CF Medium Density Polyethylene, Stripes
Total MDPE HT 514 Medium Density Polyethylene, Blown Film

PTOTAL761 / 130486

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.