MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes 625SQ® Nickel Alloy Sheet
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Haynes 625SQ alloy is a solid-solution strengthened superalloy. It is a modification of Haynes 625 alloy designed to enhance resistance to fatigue at temperatures up to approximately 1200°F (649°C). The alloy composition is tightly controlled to very low levels of carbon, silicon, and nitrogen. Primary melting is by vacuum induction melting, followed by consumable electrode practice using electroslag remelting. During processing, the grain size is controlled to ASTM #5 or finer. Haynes 625SQ alloy sheet and strip meet the requirements of AMS 5879 and AMS 5599 specifications. Haynes 625SQ alloy is readily fabricated and welded using practices common to Haynes 625 alloy. Haynes 625SQ alloy sheet and strip find application in aerospace, automotive, and chemical process industry bellows, expansion joints, and fabrications where fatigue resistance, strength, and corrosion resistance are required.

Data provided by the manufacturer, Haynes International, Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.44 g/cc0.305 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  497 MPa
@Temperature 760 °C
72100 psi
@Temperature 1400 °F
AMS 5879
 646 MPa
@Temperature 705 °C
93700 psi
@Temperature 1300 °F
AMS 5879
 776 MPa
@Temperature 425 °C
113000 psi
@Temperature 797 °F
AMS 5879
 776 MPa
@Temperature 540 °C
113000 psi
@Temperature 1000 °F
AMS 5879
 787 MPa
@Temperature 650 °C
114000 psi
@Temperature 1200 °F
AMS 5879
 809 MPa
@Temperature 315 °C
117000 psi
@Temperature 599 °F
AMS 5879
 895 MPa
@Temperature 25.0 °C
130000 psi
@Temperature 77.0 °F
AMS 5879
Tensile Strength, Yield  306 MPa
@Strain 0.2 %,
Temperature 705 °C
44400 psi
@Strain 0.2 %,
Temperature 1300 °F
AMS 5879
 323 MPa
@Strain 0.2 %,
Temperature 650 °C
46800 psi
@Strain 0.2 %,
Temperature 1200 °F
AMS 5879
 339 MPa
@Strain 0.2 %,
Temperature 425 °C
49200 psi
@Strain 0.2 %,
Temperature 797 °F
AMS 5879
 344 MPa
@Strain 0.2 %,
Temperature 540 °C
49900 psi
@Strain 0.2 %,
Temperature 1000 °F
AMS 5879
 353 MPa
@Strain 0.2 %,
Temperature 315 °C
51200 psi
@Strain 0.2 %,
Temperature 599 °F
AMS 5879
 452 MPa
@Strain 0.2 %,
Temperature 25.0 °C
65600 psi
@Strain 0.2 %,
Temperature 77.0 °F
AMS 5879
 3223 MPa
@Strain 0.2 %,
Temperature 760 °C
467500 psi
@Strain 0.2 %,
Temperature 1400 °F
AMS 5879
Elongation at Break  51.7 %
@Temperature 25.0 °C
51.7 %
@Temperature 77.0 °F
2-inch (51 mm) sample; AMS 5879
 60.9 %
@Temperature 425 °C
60.9 %
@Temperature 797 °F
2-inch (51 mm) sample; AMS 5879
 64.1 %
@Temperature 315 °C
64.1 %
@Temperature 599 °F
2-inch (51 mm) sample; AMS 5879
 81.4 %
@Temperature 650 °C
81.4 %
@Temperature 1200 °F
2-inch (51 mm) sample; AMS 5879
 88.8 %
@Temperature 760 °C
88.8 %
@Temperature 1400 °F
2-inch (51 mm) sample; AMS 5879
 90.5 %
@Temperature 540 °C
90.5 %
@Temperature 1000 °F
2-inch (51 mm) sample; AMS 5879
 103.9 %
@Temperature 705 °C
103.9 %
@Temperature 1300 °F
2-inch (51 mm) sample; AMS 5879
Modulus of Elasticity  126 GPa
@Temperature 1000 °C
18300 ksi
@Temperature 1830 °F
Dynamic
 142 GPa
@Temperature 900 °C
20600 ksi
@Temperature 1650 °F
Dynamic
 153 GPa
@Temperature 800 °C
22200 ksi
@Temperature 1470 °F
Dynamic
 163 GPa
@Temperature 700 °C
23600 ksi
@Temperature 1290 °F
Dynamic
 171 GPa
@Temperature 600 °C
24800 ksi
@Temperature 1110 °F
Dynamic
 186 GPa
@Temperature 400 °C
27000 ksi
@Temperature 752 °F
Dynamic
 199 GPa
@Temperature 200 °C
28900 ksi
@Temperature 392 °F
Dynamic
 208 GPa
@Temperature 20.0 °C
30200 ksi
@Temperature 68.0 °F
Dynamic
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.000134 ohm-cm
@Temperature 200 °C
0.000134 ohm-cm
@Temperature 392 °F
 0.0001348 ohm-cm
@Temperature 1000 °C
0.0001348 ohm-cm
@Temperature 1830 °F
 0.0001356 ohm-cm
@Temperature 400 °C
0.0001356 ohm-cm
@Temperature 752 °F
 0.0001356 ohm-cm
@Temperature 900 °C
0.0001356 ohm-cm
@Temperature 1650 °F
 0.0001365 ohm-cm
@Temperature 800 °C
0.0001365 ohm-cm
@Temperature 1470 °F
 0.0001375 ohm-cm
@Temperature 700 °C
0.0001375 ohm-cm
@Temperature 1290 °F
 0.0001379 ohm-cm
@Temperature 600 °C
0.0001379 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  14.2 µm/m-°C
@Temperature 20.0 - 500 °C
7.89 µin/in-°F
@Temperature 68.0 - 932 °F
 14.8 µm/m-°C
@Temperature 20.0 - 600 °C
8.22 µin/in-°F
@Temperature 68.0 - 1110 °F
 15.4 µm/m-°C
@Temperature 20.0 - 700 °C
8.56 µin/in-°F
@Temperature 68.0 - 1290 °F
 16.1 µm/m-°C
@Temperature 20.0 - 800 °C
8.94 µin/in-°F
@Temperature 68.0 - 1470 °F
 16.8 µm/m-°C
@Temperature 20.0 - 900 °C
9.33 µin/in-°F
@Temperature 68.0 - 1650 °F
 17.4 µm/m-°C
@Temperature 20.0 - 1000 °C
9.67 µin/in-°F
@Temperature 68.0 - 1830 °F
Thermal Conductivity  15.3 W/m-K
@Temperature 400 °C
106 BTU-in/hr-ft²-°F
@Temperature 752 °F
 18.3 W/m-K
@Temperature 600 °C
127 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 19.8 W/m-K
@Temperature 700 °C
137 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 21.5 W/m-K
@Temperature 800 °C
149 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 23.4 W/m-K
@Temperature 900 °C
162 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 25.6 W/m-K
@Temperature 1000 °C
178 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1290 - 1350 °C2350 - 2460 °F
Solidus 1290 °C2350 °F
Liquidus <= 1350 °C<= 2460 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature >= 871 °C>= 1600 °FBright Anneal; AMS 5879
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.40 %<= 0.40 %
Carbon, C <= 0.030 %<= 0.030 %
Cb + Ta 3.7 %3.7 %
Chromium, Cr 21 %21 %
Cobalt, Co <= 1.0 %<= 1.0 %
Iron, Fe <= 5.0 %<= 5.0 %
Manganese, Mn <= 0.50 %<= 0.50 %
Molybdenum, Mo 9.0 %9.0 %
Nickel, Ni >= 62 %>= 62 %as balance
Nitrogen, N <= 0.020 %<= 0.020 %
Silicon, Si <= 0.15 %<= 0.15 %
Titanium, Ti <= 0.40 %<= 0.40 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
439 Ferritic Stainless Steel (UNS S43900)
Special Metals INCONEL® Alloy 718
Haynes 625 alloy, 0% cold reduction
ATI Allvac® 718 Nickel Superalloy, Heat Treatment: 982°C (1800°F) + Age
Aluminum C355.0-T6, Sand Cast

NHAY996 / 162659

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.