MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Bohler-Uddeholm BÖHLER W360 ISOBLOC® Hot Work Tool Steel
Categories: Metal; Ferrous Metal; Tool Steel; Hot Work Steel

Material Notes: BÖHLER W360 ISOBLOC was developed as a tool steel for dies and punches in warm and hot forging. The steel can be used for a variety of applications where hardness and toughness are required. Properties
  • High hardness (recommended in use: 52 – 57 HRC)
  • Exceptional toughness
  • High temper resistance
  • Good thermal conductivity
  • Can be cooled with water
  • Homogeneous microstructure
Applications and uses
  • Dies and punches in warm and hot forging
  • Tooling for high speed presses
  • Toughness-critical cold work applications
  • Extrusion tooling, e.g. dies
  • Core pins and inserts in die-casting dies
  • Specific applications in the plastic processing sector

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.60 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 52 - 57typical range of application
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000590 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.1 µm/m-°C
@Temperature 20.0 - 100 °C
 11.5 µm/m-°C
@Temperature 20.0 - 200 °C
 11.9 µm/m-°C
@Temperature 20.0 - 300 °C
 12.3 µm/m-°C
@Temperature 20.0 - 400 °C
 12.8 µm/m-°C
@Temperature 20.0 - 500 °C
 13.2 µm/m-°C
@Temperature 20.0 - 600 °C
 13.6 µm/m-°C
@Temperature 20.0 - 700 °C
Thermal Conductivity 31.5 W/m-K
@Temperature 100 °C
 31.9 W/m-K
@Temperature 500 °C
 32.3 W/m-K
@Temperature 200 °C
 32.5 W/m-K
@Temperature 400 °C
 32.6 W/m-K
@Temperature 300 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.50 %
Chromium, Cr 4.5 %
Iron, Fe 91 %As Balance
Manganese, Mn 0.25 %
Molybdenum, Mo 3.0 %
Silicon, Si 0.20 %
Vanadium, V 0.55 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type H21 Tool Steel
Bohler-Uddeholm AISI D2 Cold Work Tool Steel
Bohler-Uddeholm BÖHLER W302 SUPERIOR® Premium H13 Tool Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPERIOR (Premium AISI H13) Hot Work Tool Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPREME (Premium AISI H13) Hot Work Tool Steel

NBUCOR50 / 98129

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.