MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

NOVA Chemicals Sclair® EX-IG454-A01 ASTute PE Injection Molding Resin  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Injection Molded

Material Notes: Superior stiffness allows for part thinwalling and improved stack strength, Low viscosity for exceptional processability, shorter cycle times, and energy savings, Exceptional physical properties provide impact resistance for demanding applications, Low warpage for improved part quality and reliability

Applications: Pails, Totes, Storage bins, Crates

Additives: Antioxidants

Information provided by NOVA Chemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.954 g/cc0.0345 lb/in³ASTM D792
ESCR 100% Igepal® <= 10 hour<= 10 hourCondition B; ASTM D1693
Melt Flow 9.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
9.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6666ASTM D2240
Tensile Strength, Ultimate 16.0 MPa2320 psi50 mm/min; ASTM D638
Tensile Strength, Yield 22.3 MPa3230 psi50 mm/min; ASTM D638
Elongation at Break 650 %650 %50 mm/min; ASTM D638
Elongation at Yield 9.0 %9.0 %50 mm/min; ASTM D638
Flexural Modulus, 1% Secant 960 MPa139000 psiASTM D790
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 128 °C262 °FASTM D1525

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PNOVA113 / 55014

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.