MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics Kaowool Moldable AR Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: RCF. Kaowool Moldable AR is specially formulated to provide a very strong and hard material that is nonwetting to molten aluminum. It is an ideal material for use in troughs and launders.

Applications:

  • Reheat Furnaces
  • Forge Furnaces
  • Heat-treating
  • Annealing furnaces
  • Kilns

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.602 - 1.683 g/ccwet
 0.881 - 0.962 g/cc
@Temperature 110 °C
dried
 
Mechanical PropertiesOriginal ValueComments
Modulus of Rupture 0.00299 GPa
@Temperature 538 °C
dried
 0.00302 GPa
@Temperature 110 °C
dried
 0.00305 GPa
@Temperature 816 °C
dried
 0.00321 GPa
@Temperature 982 °C
dried
Compressive Strength 2.07 MPa
@Temperature 110 °C
at 5% deformation, dried
 2.07 MPa
@Temperature 538 °C
at 5% deformation, dried
 2.07 MPa
@Temperature 816 °C
at 5% deformation, dried
 2.07 MPa
@Temperature 982 °C
at 5% deformation, dried
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.140 W/m-K
@Temperature 538 °C
ASTM C201
 0.190 W/m-K
@Temperature 816 °C
ASTM C201
 1.00 W/m-K
@Temperature 260 °C
ASTM C201
Maximum Service Temperature, Air <= 982 °CContinuous Use
Shrinkage 1.0 %
@Treatment Temp. 110 °C,
Time 86400 sec
 1.5 %
@Treatment Temp. 260 °C,
Time 86400 sec
 2.3 %
@Treatment Temp. 538 °C,
Time 86400 sec
 2.3 %
@Treatment Temp. 816 °C,
Time 86400 sec
 3.1 %
@Treatment Temp. 982 °C,
Time 86400 sec
 
Processing PropertiesOriginal ValueComments
Shelf Life 6.00 Month
 
Component Elements PropertiesOriginal ValueComments
Al2O3 29 - 32 %
Other 3.0 - 5.0 %
SiO2 64 - 67 %
 
Descriptive Properties
Classification Temperature (°C)982
Colorlight brown

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Modified ETFE, Unreinforced
Mocom (ALBIS) Tedur® L 9107-1 S Polyphenylene Sulfide
ESK Ceramics PolyCeram® TRIBO220 Polymer matrix composite
ESK Ceramics PolyCeram® TRIBO140 Polymer matrix composite
CHT Group QSil 553LV Addition Cure Potting Material

CMORF6067 / 202851

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.