MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

Epoxies, Etc 10-3003 Epoxy Adhesive
Categories: Polymer; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: 10-3003 is a new high bond strength epoxy adhesive formulated for ease in handling and convenience for the end user. This system has a non-critical mix ratio and adjustable flexibility. 10-3003 is also very safe to use due to the absence of harmful solvents and toxic chemicals in the formulation. 10-3003 yields high peel strength and excellent tensile strength. It also has outstanding thermal shock, impact and vibration resistance. This high performance epoxy adhesive exhibits outstanding physical, thermal, and electrical insulation properties. 10-3004 NC is available as a very low viscosity version of 10-3003. 10-3002 is available as a higher viscosity version of 10-3003.and polyol offer good low viscosity handling characteristics and turn thixotropic upon mixing.

Features:

  • Non-critical mix ratio
  • Excellent chemical resistance
  • Ability to adjust flexibility of bond line
  • Very good operating temperature range
  • Outstanding thermal shock resistance

Information provided by Epoxies, Etc

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.960 g/cc0.960 g/ccCatalyst
 1.17 g/cc1.17 g/ccResin
Viscosity 1000 cP1000 cP10-3004NC Resin
 1200 cP1200 cP10-3002 Resin
 4500 cP4500 cP10-3002 Hardener
 5400 cP5400 cP10-3004 NC Mixed
 6000 cP6000 cP10-3003 Hardener
 12000 - 15000 cP12000 - 15000 cP10-3003 Resin
 15000 cP15000 cP10-3003 Mixed
 15000 cP15000 cP10-3004 Hardener
 70000 cP70000 cP10-3002 Mixed
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 72.4 MPa10500 psi
Flexural Strength 352 MPa51000 psi
Adhesive Bond Strength 5.17 MPa750 psiPVC to PVC
 8.27 MPa1200 psiNylon to Nylon
 10.3 MPa1500 psiCopper to Copper
 12.8 MPa1850 psiTeflon*to Aluminum
 17.9 MPa2600 psiBrass to Brass
 20.7 MPa3000 psiSteel to Steel
 22.8 MPa3300 psiAluminum to Aluminum
Izod Impact, Notched 2.14 J/cm4.00 ft-lb/in
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.10e+15 ohm-cm1.10e+15 ohm-cm
Dielectric Constant 3.113.1110E3 cycles
Dielectric Strength 21.7 kV/mm550 kV/in
Dissipation Factor 0.0200.02010E3 cycles
 
Thermal PropertiesMetricEnglishComments
CTE, linear 50.0 µm/m-°C27.8 µin/in-°F
Thermal Conductivity 0.430 W/m-K2.98 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 125 °C257 °F
Minimum Service Temperature, Air -50.0 °C-58.0 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  15.0 - 30.0 min
@Temperature 93.0 - 104 °C
0.250 - 0.500 hour
@Temperature 199 - 219 °F
 30.0 - 60.0 min
@Temperature 66.0 - 71.0 °C
0.500 - 1.00 hour
@Temperature 151 - 160 °F
 1440 min
@Temperature 25.0 °C
24.0 hour
@Temperature 77.0 °F
Pot Life 90.0 min
@Load 0.100 kg
90.0 min
@Load 0.221 lb
 
Descriptive Properties
ColorClear

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PFEPOX070 / 316747

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.