MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Pressure Seal 14801 Chlorosulfonated
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 14801 is a 70 durometer black colored general purpose Hypalonelastomer. It has good physicals and exhibits good resistance to synthetic lubricating oils.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 CE 715; 3 CE 715 B15

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.49 g/cc1.49 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7171
 50
@Treatment Temp. 125 °C,
Time 252000 sec
50
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #3
 59
@Treatment Temp. 23.0 °C,
Time 252000 sec
59
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel B
 67
@Treatment Temp. 150 °C,
Time 252000 sec
67
@Treatment Temp. 302 °F,
Time 70.0 hour
Service Fluid 100
 67
@Treatment Temp. 125 °C,
Time 252000 sec
67
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged
 69
@Treatment Temp. 23.0 °C,
Time 252000 sec
69
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
 71
@Treatment Temp. 100 °C,
Time 252000 sec
71
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 73
@Treatment Temp. 125 °C,
Time 252000 sec
73
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #1
 81
@Treatment Temp. 125 °C,
Time 252000 sec
81
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 84
@Treatment Temp. 150 °C,
Time 252000 sec
84
@Treatment Temp. 302 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 84
@Treatment Temp. 150 °C,
Time 252000 sec
84
@Treatment Temp. 302 °F,
Time 70.0 hour
Heat Aged
Tensile Strength 21.73 MPa3152 psi
 6.846 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
992.9 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
Heat Aged
 6.846 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
992.9 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 10.127 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
1468.8 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel B
 15.278 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
2215.9 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #3
 19.255 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
2792.7 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
 19.776 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
2868.3 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
Service Fluid 100
 22.232 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
3224.5 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 22.949 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
3328.5 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #1
 23.384 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
3391.6 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 23.384 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
3391.6 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged
Elongation, Ultimate 259 %259 %
 50 %
@Treatment Temp. 150 °C,
Time 252000 sec
50 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Heat Aged
 50 %
@Treatment Temp. 150 °C,
Time 252000 sec
50 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 129 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
129 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel B
 175.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
175.1 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 175.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
175.1 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged
 196.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
196.1 %
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #1
 212.9 %
@Treatment Temp. 125 °C,
Time 252000 sec
212.9 %
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #3
 220.9 %
@Treatment Temp. 100 °C,
Time 252000 sec
220.9 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 229.5 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
229.5 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
 246.05 %
@Treatment Temp. 150 °C,
Time 252000 sec
246.05 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Service Fluid 100
100% Modulus 4.99 MPa724 psi
Tear Strength 35.8 kN/m204 pliDie B
Compression Set  15.3 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
15.3 %
@Treatment Temp. 158 °F,
Time 22.0 hour
Solid
 73.6 %
@Treatment Temp. 125 °C,
Time 79200 sec
73.6 %
@Treatment Temp. 257 °F,
Time 22.0 hour
Solid
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -46.1 °C-51.0 °F
Shrinkage  -5.10 %
@Treatment Temp. 150 °C,
Time 252000 sec
-5.10 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, Heat Aged
 -5.10 %
@Treatment Temp. 150 °C,
Time 252000 sec
-5.10 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, Heat Aged, Test Tube Method
 -4.00 %
@Treatment Temp. 125 °C,
Time 252000 sec
-4.00 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Volume, Heat Aged, Test Tube Method
 -4.00 %
@Treatment Temp. 125 °C,
Time 252000 sec
-4.00 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Weight, Heat Aged
 2.5 %
@Treatment Temp. 125 °C,
Time 252000 sec
2.5 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Volume, ASTM Oil #1
 7.7 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
7.7 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel A
 9.2 %
@Treatment Temp. 100 °C,
Time 252000 sec
9.2 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Volume, Distilled water aged
 10.5 %
@Treatment Temp. 150 °C,
Time 252000 sec
10.5 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, Service Fluid 100
 53.5 %
@Treatment Temp. 125 °C,
Time 252000 sec
53.5 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Volume, ASTM Oil #3
 53.8 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
53.8 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel B
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPRESL093 / 318303

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.