Physical Properties | Metric | English | Comments |
---|
Density | 8.73 g/cc | 0.315 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength | 1240 MPa | 180000 psi |
Tensile Strength, Yield | 1110 MPa @Strain 0.2 % | 161000 psi @Strain 0.2 % |
Elongation at Break | 10 % | 10 % |
Modulus of Elasticity | 165 GPa @Temperature 700 °C | 23900 ksi @Temperature 1290 °F |
| 173 GPa @Temperature 600 °C | 25100 ksi @Temperature 1110 °F |
| 183 GPa @Temperature 500 °C | 26500 ksi @Temperature 932 °F |
| 185 GPa @Temperature 400 °C | 26800 ksi @Temperature 752 °F |
| 193 GPa @Temperature 300 °C | 28000 ksi @Temperature 572 °F |
| 197 GPa @Temperature 200 °C | 28600 ksi @Temperature 392 °F |
| 205 GPa @Temperature 100 °C | 29700 ksi @Temperature 212 °F |
| 207 GPa @Temperature 20.0 °C | 30000 ksi @Temperature 68.0 °F |
Poissons Ratio | 0.33 @Temperature 600 °C | 0.33 @Temperature 1110 °F |
| 0.34 @Temperature 400 °C | 0.34 @Temperature 752 °F |
| 0.34 @Temperature 20.0 °C | 0.34 @Temperature 68.0 °F |
| 0.35 @Temperature 700 °C | 0.35 @Temperature 1290 °F |
| 0.37 @Temperature 500 °C | 0.37 @Temperature 932 °F |
| 0.37 @Temperature 100 °C | 0.37 @Temperature 212 °F |
| 0.37 @Temperature 200 °C | 0.37 @Temperature 392 °F |
| 0.38 @Temperature 300 °C | 0.38 @Temperature 572 °F |
Fatigue Strength | 410 MPa @# of Cycles 1.00e+7 | 59500 psi @# of Cycles 1.00e+7 |
| 500 MPa @# of Cycles 1.00e+6 | 72500 psi @# of Cycles 1.00e+6 |
| 690 MPa @# of Cycles 100000 | 100000 psi @# of Cycles 100000 |
Shear Modulus | 61.0 GPa @Temperature 700 °C | 8850 ksi @Temperature 1290 °F |
| 65.0 GPa @Temperature 600 °C | 9430 ksi @Temperature 1110 °F |
| 67.0 GPa @Temperature 500 °C | 9720 ksi @Temperature 932 °F |
| 69.0 GPa @Temperature 400 °C | 10000 ksi @Temperature 752 °F |
| 70.0 GPa @Temperature 300 °C | 10200 ksi @Temperature 572 °F |
| 72.0 GPa @Temperature 200 °C | 10400 ksi @Temperature 392 °F |
| 75.0 GPa @Temperature 100 °C | 10900 ksi @Temperature 212 °F |
| 77.0 GPa @Temperature 20.0 °C | 11200 ksi @Temperature 68.0 °F |
Impact Test | 404 J @Temperature -196 °C | 298 ft-lb @Temperature -321 °F |
| 405 J @Temperature 20.0 °C | 299 ft-lb @Temperature 68.0 °F |
| 2.70 J @Temperature -196 °C, Treatment Temp. 980 °C | 1.99 ft-lb @Temperature -321 °F, Treatment Temp. 1800 °F |
| 2.70 J @Temperature 20.0 °C, Treatment Temp. 980 °C | 1.99 ft-lb @Temperature 68.0 °F, Treatment Temp. 1800 °F |
| 3.40 J @Temperature -196 °C, Treatment Temp. 870 °C | 2.51 ft-lb @Temperature -321 °F, Treatment Temp. 1600 °F |
| 8.10 J @Temperature 20.0 °C, Treatment Temp. 870 °C | 5.97 ft-lb @Temperature 68.0 °F, Treatment Temp. 1600 °F |
| 12.2 J @Temperature -196 °C, Treatment Temp. 760 °C | 9.00 ft-lb @Temperature -321 °F, Treatment Temp. 1400 °F |
| 25.1 J @Temperature 20.0 °C, Treatment Temp. 760 °C | 18.5 ft-lb @Temperature 68.0 °F, Treatment Temp. 1400 °F |
| 400 J @Temperature 20.0 °C, Treatment Temp. 540 °C | 295 ft-lb @Temperature 68.0 °F, Treatment Temp. 1000 °F |
| 401 J @Temperature 20.0 °C, Treatment Temp. 650 °C | 296 ft-lb @Temperature 68.0 °F, Treatment Temp. 1200 °F |
| 403 J @Temperature -196 °C, Treatment Temp. 650 °C | 297 ft-lb @Temperature -321 °F, Treatment Temp. 1200 °F |
| 405 J @Temperature -196 °C, Treatment Temp. 540 °C | 299 ft-lb @Temperature -321 °F, Treatment Temp. 1000 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0001238 ohm-cm | 0.0001238 ohm-cm |
Magnetic Permeability | 1.0001 | 1.0001 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 11.97 µm/m-°C @Temperature 21.0 - 100 °C | 6.650 µin/in-°F @Temperature 69.8 - 212 °F |
| 12.22 µm/m-°C @Temperature 21.0 - 200 °C | 6.789 µin/in-°F @Temperature 69.8 - 392 °F |
| 12.56 µm/m-°C @Temperature 21.0 - 300 °C | 6.978 µin/in-°F @Temperature 69.8 - 572 °F |
| 12.87 µm/m-°C @Temperature 21.0 - 400 °C | 7.150 µin/in-°F @Temperature 69.8 - 752 °F |
| 13.01 µm/m-°C @Temperature 21.0 - 500 °C | 7.228 µin/in-°F @Temperature 69.8 - 932 °F |
| 13.18 µm/m-°C @Temperature 21.0 - 600 °C | 7.322 µin/in-°F @Temperature 69.8 - 1110 °F |
Specific Heat Capacity | 0.364 J/g-°C @Temperature -15.0 °C | 0.0870 BTU/lb-°F @Temperature 5.00 °F |
| 0.373 J/g-°C @Temperature 20.0 °C | 0.0891 BTU/lb-°F @Temperature 68.0 °F |
| 0.389 J/g-°C @Temperature 100 °C | 0.0930 BTU/lb-°F @Temperature 212 °F |
| 0.410 J/g-°C @Temperature 200 °C | 0.0980 BTU/lb-°F @Temperature 392 °F |
| 0.431 J/g-°C @Temperature 300 °C | 0.103 BTU/lb-°F @Temperature 572 °F |
| 0.456 J/g-°C @Temperature 400 °C | 0.109 BTU/lb-°F @Temperature 752 °F |
| 0.477 J/g-°C @Temperature 500 °C | 0.114 BTU/lb-°F @Temperature 932 °F |
| 0.498 J/g-°C @Temperature 600 °C | 0.119 BTU/lb-°F @Temperature 1110 °F |
| 0.519 J/g-°C @Temperature 700 °C | 0.124 BTU/lb-°F @Temperature 1290 °F |
Thermal Conductivity | 9.80 W/m-K @Temperature 25.0 °C | 68.0 BTU-in/hr-ft²-°F @Temperature 77.0 °F |
| 12.8 W/m-K @Temperature 200 °C | 88.8 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 16.6 W/m-K @Temperature 400 °C | 115 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 21.4 W/m-K @Temperature 600 °C | 149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 25.3 W/m-K @Temperature 800 °C | 176 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 29.6 W/m-K @Temperature 1000 °C | 205 BTU-in/hr-ft²-°F @Temperature 1830 °F |
| 32.6 W/m-K @Temperature 1150 °C | 226 BTU-in/hr-ft²-°F @Temperature 2100 °F |
Melting Point | 1338 - 1380 °C | 2440 - 2520 °F |
Solidus | 1338 °C | 2440 °F |
Liquidus | 1380 °C | 2520 °F |
|
Processing Properties | Metric | English | Comments |
---|
Annealing Temperature | 1180 - 1200 °C | 2160 - 2190 °F |
Hot-Working Temperature | 870 - 1230 °C | 1600 - 2250 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.010 % | <= 0.010 % |
Chromium, Cr | 19 - 23 % | 19 - 23 % |
Iron, Fe | <= 2.0 % | <= 2.0 % |
Manganese, Mn | <= 0.75 % | <= 0.75 % |
Molybdenum, Mo | 15 - 17 % | 15 - 17 % |
Nickel, Ni | 52.5 - 63 % | 52.5 - 63 % |
Phosphorus, P | <= 0.040 % | <= 0.040 % |
Silicon, Si | <= 0.080 % | <= 0.080 % |
Sulfur, S | <= 0.020 % | <= 0.020 % |
Titanium, Ti | 0.020 - 0.25 % | 0.020 - 0.25 % |
Tungsten, W | 3.0 - 4.4 % | 3.0 - 4.4 % |