MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Trinseo Magnum™ 8391 MED Acrylonitrile Butadiene Styrene (ABS) Resin
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes: MAGNUM™ 8391 MED ABS combines an excellent gloss appearance with high flow and medium impact performance. The mass (continuous process) ABS technology ensures an ABS resin that combines excellent processability with a stable light base color that is ideal for self-coloring. MAGNUM 8391 MED natural resin has undergone biocompatibility testing based on ISO 10993 (Biological Evaluation of Medical Devices) and is suitable for use in approved medical applications.

Applications:

  • Medical Applications

Information provided by Trinseo.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ASTM D792
Apparent Bulk Density 0.650 g/cc0.0235 lb/in³ISO 60
Linear Mold Shrinkage, Flow 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inISO 294-4
Melt Flow  8.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
8.0 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 28 g/10 min
@Load 10.0 kg,
Temperature 220 °C
28 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 108108ASTM D785
Tensile Strength at Break 35.0 MPa5080 psiInjection Molded, 50 mm/min; ASTM D638
Tensile Strength, Yield 48.0 MPa6960 psiInjection Molded, 50 mm/min; ASTM D638
 45.0 MPa
@Thickness 3.20 mm
6530 psi
@Thickness 0.126 in
Injection Molded; ISO 527-2/50
 47.0 MPa
@Thickness 3.20 mm
6820 psi
@Thickness 0.126 in
Injection Molded; ISO 527-2/100
Tensile Modulus 2.34 GPa
@Thickness 3.20 mm
339 ksi
@Thickness 0.126 in
Injection Molded; ISO 527-2
Flexural Strength 75.0 MPa10900 psi1.3 mm/min; ASTM D790
 70.0 MPa
@Thickness 3.20 mm
10200 psi
@Thickness 0.126 in
Injection Molded, 2.0 mm/min, 3-points; ISO 178
Flexural Modulus 2.40 GPa348 ksiInjection Molded, 2.0 mm/min, 3-points; ISO 178
 2.48 GPa360 ksi1.3 mm/min; ASTM D790
Izod Impact, Notched 2.30 J/cm4.31 ft-lb/inASTM D256
Izod Impact, Notched (ISO)  9.00 kJ/m²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
Injection Molded; ISO 180/A
 19.0 kJ/m²
@Temperature 23.0 °C
9.04 ft-lb/in²
@Temperature 73.4 °F
Injection Molded; ISO 180/A
Charpy Impact, Notched  0.900 J/cm²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
Injection Molded; ISO 179/1eA
 1.90 J/cm²
@Temperature 23.0 °C
9.04 ft-lb/in²
@Temperature 73.4 °F
Injection Molded; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 87.0 °C189 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 74.0 °C165 °FUnannealed; ASTM D648
 95.0 °C203 °FAnnealed; ISO 75-2/A
Vicat Softening Point 95.0 °C203 °FISO 306/B50
 99.0 °C210 °FRate B (120°C/h), Loading 1 (10 N); ASTM D1525
Flammability, UL94  HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Trinseo MAGNUM™ 8391 Acrylonitrile Butadiene Styrene (ABS) Resin
Trinseo MAGNUM™ 3904 Acrylonitrile Butadiene Styrene (ABS) Resin
Trinseo Magnum™ 9010 ABS, High Gloss
INEOS Styrolution Terluran® GP-35 ABS
Ineos ABS Lustran® 308 ABS, Medical Grade

PDWST078 / 142287

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.