MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AFE Technologies Cronite 37Ni/18Cr/Nb No. HR32
Categories: Metal; Superalloy; Iron Base

Material Notes: High temperature nickel alloy castings. Applications include heat treatment and handling products, furnace products, tubes, power generation, and petrochemical industries.

Information provided by AFE Technologies/North American Cronite, Inc.

Key Words: Cronite 37/18 Nb; Werkstoff 1.4849
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 480 MPaAs Cast
Tensile Strength, Yield 250 MPaAs Cast
Elongation at Break 8.0 %As Cast; 5.65 A0.5
Rupture Strength 3.40 MPa
@Temperature 1150 °C,
Time 3.60e+7 sec
Stress Rupture
 5.30 MPa
@Temperature 1100 °C,
Time 3.60e+7 sec
Stress Rupture
 8.00 MPa
@Temperature 1050 °C,
Time 3.60e+7 sec
Stress Rupture
 12.0 MPa
@Temperature 1000 °C,
Time 3.60e+7 sec
Stress Rupture
 18.0 MPa
@Temperature 950 °C,
Time 3.60e+7 sec
Stress Rupture
 25.0 MPa
@Temperature 900 °C,
Time 3.60e+7 sec
Stress Rupture
 34.0 MPa
@Temperature 850 °C,
Time 3.60e+7 sec
Stress Rupture
 45.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
Stress Rupture
 59.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
Stress Rupture
 78.0 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
Stress Rupture
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.40 %
Chromium, Cr 18 %
Iron, Fe 40.6 %As Remainder
Manganese, Mn 1.0 %
Nickel, Ni 37 %
Niobium, Nb (Columbium, Cb) 1.5 %
Silicon, Si 1.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AFE Technologies Cronite 37Ni/18Cr No. HR5
Alloy Wire International RW 45 Ni-Cu Resistance Wire
Constantan Thermocouple Wire
Cunife® Hard Magnetic Alloy
Eagle Brass 752 Nickel Silver 18%, Hard

NCRON03 / 15988

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.