MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LCY Globalene TPV 1040D BK Thermoplastic Vulcanized Elastomers
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: A high hardness, multi-purpose thermoplastic elastomer featuring excellent compression set and high temperature performance. Globalene TPV 1040D BK can be processed by extrusion or molding for applications such as weatherstrip profile, seals, window gaskets and other soft touch articles.

Attributes:

  • Globalene TPV 1000 series is a fully vulcanized Thermoplastic Elastomers containing EPDM and PP.
  • It is designed for applications requiring long term sealing performance even at elevated temperatures.
  • Suitable for injection molding, profile extrusion or re-compounding for plastics modification.
  • Conventional thermoplastic processing equipment can be used.
Applications: Globalene TPV has quality sealing property, good chemical and weathering resistance and electrical property that is suitable to replace main stream TPV, thermoset EPDM rubber, Styrene based TPEs, flexible PVC and other TPEs. It is an excellent choice for applications requiring flexibility in the following markets: automotive parts, appliance, business machines, construction, consumer products, and electronics.

Information provided by LCY Chemical Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.960 g/ccISO 1183
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 41
@Time 15.0 sec
Injection Molded; ISO 868
Tensile Strength at Break 20.0 MPa500 mm/min; ISO 37
Elongation at Break 550 %500 mm/min; ISO 37
100% Modulus 10.0 MPa500 mm/min; ISO 37
Tear Strength 64.0 kN/m500 mm/min; ISO 34-1
Compression Set 54 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 79 %
@Temperature 125 °C,
Time 252000 sec
ISO 815
 
Thermal PropertiesOriginal ValueComments
Melting Point 160 °C
Brittleness Temperature -45.0 °CISO 812
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 180 - 190 °CInjection
Middle Barrel Temperature 200 - 220 °CInjection
Front Barrel Temperature 200 - 220 °CInjection
Nozzle Temperature 200 - 220 °CInjection
Zone 1 180 °CExtrusion
Zone 2 190 °CExtrusion
Zone 3 200 °CExtrusion
Zone 4 210 °CExtrusion
Zone 5 210 °CExtrusion
Die Temperature 210 - 220 °CExtrusion
Melt Temperature 180 - 220 °CExtrusion
 200 - 220 °CInjection
Mold Temperature 30.0 - 55.0 °CInjection
Roll Temperature 20.0 - 50.0 °CExtrusion
Injection Pressure 4.80 - 6.90 MPaInjection
Hold Pressure 2.10 - 4.10 MPaInjection
Back Pressure 10.0 - 150 psiInjection
Vent Depth 0.00100 inInjection
Screw Speed 100 - 200 rpmInjection
Shelf Life 36.0 Month
 
Descriptive Properties
Cooling Time15-30 secInjection
Holding Time4-10 secInjection
Ozone ResistanceExcellent500 hr, 100 pphm O3 conc, ASTM D-1149
Screen Pack20-60 meshExtrusion
Screw>24:1L/D ratio
 3:1Compression ratio

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PLCY118 / 295661

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.