MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Freudenberg Sealing Technologies 75 FKM 38269 Fluoroelastomer
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: FKM 38269 is the preferred choice for standard articles such as O-rings.

FKM seals display very good resistance to media, ozone and aging. The material is also stable in fuels as well as petroleum-based oils and greases, along with aliphatic and aromatic hydrocarbons. It is unstable with regard to polar solvents (e.g. acetone, MEK and ethyl acetate), low molecular weight organic acids (formic and acetic acid), glycol-based brake fluid, ammonia gas, amines, alkalis and superheated steam.

Information provided by Freudenberg Sealing Technologies.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.08 - 2.14 g/cc
@Temperature 23.0 °C
0.0751 - 0.0773 lb/in³
@Temperature 73.4 °F
Required (not typical) value; ASTM D1817
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 70 - 80
@Temperature 23.0 °C
70 - 80
@Temperature 73.4 °F
Required (not typical) value; DIN ISO 7619-1
Tensile Strength 23.7 MPa
@Temperature 23.0 °C
3440 psi
@Temperature 73.4 °F
DIN 53504, S2
Elongation at Break 240 %
@Temperature 23.0 °C
240 %
@Temperature 73.4 °F
DIN 53504, S2
Compression Set 19 %
@Temperature 200 °C,
Time 86400 sec
19 %
@Temperature 392 °F,
Time 24.0 hour
ASTM D395, B
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 200 °C392 °F
Minimum Service Temperature, Air -25.0 °C-13.0 °F
 -15.0 °C5.00 °FASTM D1329, TR10
 
Descriptive Properties
Colorblack
Cross-linkingperoxidic

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PFREU9146 / 293660

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.