Physical Properties | Original Value | Comments |
---|
Density | 1.46 g/cc @Temperature 23.0 °C |
Filler Content | 40 % |
Moisture Absorption | 1.5 - 1.8 % @Temperature 70.0 °C |
Water Absorption at Saturation | 5.2 - 5.7 % @Time 82800 sec |
Linear Mold Shrinkage, Flow | 0.0010 cm/cm |
Linear Mold Shrinkage, Transverse | 0.0090 cm/cm |
Spiral Flow | 54.0 cm |
|
Mechanical Properties | Original Value | Comments |
---|
Ball Indentation Hardness | 250 MPa |
Tensile Strength at Break | 205 MPa |
| 102.5 MPa @Treatment Temp. 160 - 175 °C, Time 1.80e+7 sec |
| 102.5 MPa @Treatment Temp. 130 - 150 °C, Time 7.20e+7 sec |
Elongation at Break | 3.0 % |
Tensile Modulus | 12800 MPa |
Flexural Strength | 300 MPa |
Flexural Modulus | 10300 MPa |
Charpy Impact Unnotched | 90.0 kJ/m² @Temperature -30.0 °C |
| 100 kJ/m² @Temperature 23.0 °C |
Charpy Impact, Notched | 14.0 kJ/m² @Temperature -30.0 °C |
| 17.0 kJ/m² @Temperature 23.0 °C |
|
Electrical Properties | Original Value | Comments |
---|
Volume Resistivity | 1.00e+13 ohm-cm |
Surface Resistance | 1.00e+12 ohm |
Comparative Tracking Index | 600 V |
|
Thermal Properties | Original Value | Comments |
---|
Melting Point | 220 °C |
Deflection Temperature at 0.46 MPa (66 psi) | 220 °C |
Deflection Temperature at 1.8 MPa (264 psi) | 215 °C |
Deflection Temperature at 8.0 MPa | 170 °C |
Flammability, UL94 | HB @Thickness 1.60 mm |
Glow Wire Flammability Index | 650 °C @Thickness 1.60 mm |
|
Processing Properties | Original Value | Comments |
---|
Feed Temperature | 60.0 - 80.0 °C |
Nozzle Temperature | 240 - 280 °C |
Zone 1 | 225 - 300 °C |
Zone 2 | 225 - 300 °C |
Zone 3 | 225 - 300 °C |
Zone 4 | 225 - 300 °C |
Melt Temperature | 260 - 300 °C |
Mold Temperature | 80.0 - 100 °C |
Drying Temperature | 80.0 °C |
Dry Time | 2.00 hour |
Hold Pressure | 30.0 - 80.0 MPa |
Back Pressure | 5.00 - 10.0 MPa |
|
Descriptive Properties |
---|
Rate acc. FMVSS 302 (<100/min) | Passed |
Rate acc. FMVSS 302,(<100/min) | FMVSS 302, >1 [mm] Thickness |
Resistance to Oleic acid | Pass |
Resistance to Acetaldehyde | Fail |
Resistance to Acetic Acid | Pass |
Resistance to Acetone | Pass |
Resistance to Acetonitrile | Pass |
Resistance to Acrylonitrile | Pass |
Resistance to Allyl alcohol | Fail |
Resistance to Amyl alcohol | Pass |
Resistance to Aqueous Ammonia | Pass |
Resistance to Benzene | Fail |
| Pass |
| Pass |
Resistance to Biodiesel | Pass |
Resistance to Boric acid | Fail |
| Pass |
Resistance to Brake fluid (DOT 4) | Fail |
| Pass |
Resistance to Calcium chloride, alcoholic | Fail |
Resistance to Calcium chloride, aqueous | Pass |
Resistance to Carbonic acid | Pass |
Resistance to Caustic potash solution, aqueous | Pass |
Resistance to Chlorine | Fail |
Resistance to Chlorine water | Fail |
Resistance to Chloroacetic acid | Fail |
Resistance to Chromic acid | Fail |
Resistance to Cyclohexane | Pass |
Resistance to Cyclohexanol | Pass |
Resistance to Dichloro-Acetic acid | Fail |
Resistance to Diesel fuel (DIN 51601) | Pass |
Resistance to Ethanol | Pass |
Resistance to Ethylene glycol/water | Fail |
Resistance to Formaldehyde, aqueous | Pass |
Resistance to Formic acid | Fail |
Resistance to Glycerin | Pass |
Resistance to Hydraulic oil H and HL (DIN 51524) | Pass |
Resistance to Hydrogen chloride, gas | Fail |
Resistance to Iso-octanol | Pass |
Resistance to Isopropanol | Pass |
Resistance to Methanol | Pass |
Resistance to Methylene chloride | Fail |
Resistance to Motor oil (SAE 10W-40) | Pass |
| Pass |
Resistance to Natural Gas | Pass |
Resistance to Nitric acid | Fail |
Resistance to Ozone | Fail |
Resistance to Phenol | Fail |
Resistance to Phosphoric acid | Fail |
Resistance to Potassium chloride, aqueous | Pass |
Resistance to Potassium permanganate, aqueous | Fail |
Resistance to Sodium chloride, aqueous | Pass |
Resistance to Sodium hydroxide solution, aqueous | Pass |
Resistance to Sodium hypochlorite, aqueous | Fail |
Resistance to Transmission oil (ATF m 1375.4) | Pass |
Resistance to Urea, aqueous | Pass |
Resistant to Carbon disulfide | Pass |
Resistant to Carbon tetrachloride | Pass |
Resistant to Citric acid | Pass |
Resistant to Ethyl acetate | Pass |
Resistant to Hydrochloric acid | Fail |
Resistant to Hydrogen peroxide | Fail |
Resistant to Seawater | Pass |
Resistant to Silicone fluid | Pass |
Resistant to Sodium hypochlorite, aqueous | Fail |
Resistant to Sulfuric acid | Fail |
| Fail |
Resistant to Super-grade petrol (DIN 51600) | Pass |
Resistant to Toluol | Pass |
Resistant to Water | Pass |
Resistant to Xylol | Pass |
Resistant to Zinc chloride, aqueous | Fail |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.