MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

DuPont Teijin Films Mylar® RL53T Polyester Packaging Film, 100 Gauge  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyester Film

Material Notes: Data provided by DuPont Packaging Polymers.

Mylar® RL53T is a biaxially oriented polyester (OPET) film with an ethylene vinyl acetate (EVA) heat seal layer. It is used as a heat sealable lidding film in packaging frozen and refrigerated foods. Mylar® RL53T is designed to produce very good heat seals to a broad range of container substrates including amorphous polyester (APET, also PETG), semicrystalline polyester (CPET), polyester coated paperboard, polyvinylchloride (PVC), polyethylene (HDPE), polypropylene (PP), and polystyrene (HIPS). Mylar® RL53T has the same type heat seal layer as Mylar® RL51T, but the seal layer is thicker than both Mylar® RL51T and Mylar® RL52T. Mylar® RL53T develops stronger seals than Mylar® RL52T to most substrates. It provides the strongest seal to polystyrene containers of all RL types. Seals made with Mylar® RL53T tend to be more ductile under refrigerated or frozen conditions versus RL33 or RL43. Mylar® RL53T is recommended for applications where light caulking is needed. Mylar® RL53T has a lower seal initiation temperature than lidding films with an amorphous polyester heat seal layer (e.g., Mylar® OL, OL2). This allows good seals to be made at higher line speeds (or using lower sealing temperatures). Mylar® RL53T has corona treatment (on the opposite side of film from the heat seal layer) to enhance printing and laminating. The film is treated to an initial dyne level of 54. The dyne level of treated lidding films may decline with storage, and in-line corona treatment may be required during subsequent printing or laminating to increase the dyne level to a value adequate to get desired ink or laminate adhesion.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.25 g/cc0.0452 lb/in³Calculated from nominal thickness and yield
Moisture Vapor Transmission 0.670 cc-mm/m²-24hr-atm1.70 cc-mil/100 in²-24hr-atmProc. E; ASTM E96
Oxygen Transmission 2.56 cc-mm/m²-24hr-atm6.50 cc-mil/100 in²-24hr-atmTested per ASTM D3985 at 22°C
Thickness 25.4 microns1.00 mil
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 110 %110 %ASTM D882
Film Elongation at Break, TD 80 %80 %ASTM D882
Secant Modulus 3.79 GPa550 ksiStiffness Modulus; ASTM D882
Tear Strength Test 1.11.1lb Graves; ASTM D1004
Film Tensile Strength at Break, MD 172 MPa24900 psiASTM D882
Film Tensile Strength at Break, TD 241 MPa35000 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 121 °C250 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature >= 177 °C>= 351 °FProduces weak seals to PP at seal temperatures below 177°C.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont™ Tedlar® TUT10BG3 UV Screening Transparent Polyvinyl Fluoride Film
DuPont™ Tedlar® TTR10BG3 Transparent Polyvinyl Fluoride Film
DuPont™ Tedlar® SP TXX10AH9 Polyvinyl Fluoride Film
DuPont Teijin Films Mylar® OL22 Polyester Film, 100 Gauge
DuPont Teijin Films Mylar® OB13AF Polyester Film, 100 Gauge

PDU7E4 / 33234

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.