MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Bohler-Uddeholm UDDEHOLM HOTVAR® Hot Work Tool Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Tool Steel; Hot Work Steel

Material Notes: Molybdenum-vanadium alloyed steel

Hotvar® is a premium hot work steel developed by Uddeholm to provide very good performance in tooling up to 1200°F (650°C). The alloying elements in Hotvar® are balanced to give high hot wear resistance and good high temperature properties. Manufactured by special techniques, Hotvar® is suitable for applications where hot wear and/or plastic deformation are the dominating failure mechanisms.

Hotvar is characterized by:

  • High hot wear resistance
  • Very good high temperature properties
  • High resistance to thermal fatigue
  • Very good temper resistance
  • Very good thermal conductivity
Applications: Uddeholm Hotvar is a hot-work tool steel suitable for applications where hot wear and/or plastic deformation are the dominating failure mechanisms. Applications and tools of especial interest:
  • Warm forging, dies and punches
  • Roll forging, rolling segments
  • Rock orbital forging, punches and dies
  • Upset forging, clamping tools
  • Progressive forging, dies
  • Axial closed die rolling, top and bottom dies
  • Cross forming, segments
  • Hot bending, tools
  • Hot calibration, tools
  • Zinc die casting, dies
  • Al-tube extrusion

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.281 lb/in³hardness of 56 HRC
 0.274 lb/in³
@Temperature 599 °C
hardness of 56 HRC
 0.277 lb/in³
@Temperature 399 °C
hardness of 56 HRC
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 210Soft annealed
Hardness, Rockwell C 54 - 58
Tensile Strength, Ultimate 305000 psihardness of 54 HRC
 320000 psihardness of 56 HRC
 335000 psihardness of 58 HRC
Tensile Strength, Yield 260000 psi
@Strain 0.2 %
hardness of 52 HRC
 265000 psi
@Strain 0.2 %
hardness of 56 HRC
 270000 psi
@Strain 0.2 %
hardness of 58 HRC
Modulus of Elasticity 30500 ksi(hardness of 56 HRC)
 20300 ksi
@Temperature 599 °C
hardness of 56 HRC
 26100 ksi
@Temperature 399 °C
hardness of 56 HRC
Charpy Impact 8.80 ft-lb
@Temperature 98.9 °C
V-notch
 12.0 ft-lb
@Temperature 399 °C
V-notch
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.00 µin/in-°F
@Temperature 399 °C
hardness of 56 HRC
 7.30 µin/in-°F
@Temperature 599 °C
hardened to 56 HRC
Thermal Conductivity 31.0 W/m-Khardness of 56 HRC
 33.0 W/m-K
@Temperature 399 °C
hardness of 56 HRC
 33.0 W/m-K
@Temperature 599 °C
hardness of 56 HRC
 
Processing PropertiesOriginal ValueComments
Processing Temperature 1920 °Fhardening temperature, then quenched in air and tempered 2 + 2 h at 1070°F (hardness = 56 HRC)
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.55 %
Chromium, Cr 2.6 %
Iron, Fe 92 %As Balance
Manganese, Mn 0.75 %
Molybdenum, Mo 2.25 %
Silicon, Si 1.0 %
Vanadium, V 0.85 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type H21 Tool Steel
AISI Type H13 Hot Work Tool Steel
Assab Steels HOTVAR Hot Work Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPERIOR (Premium AISI H13) Hot Work Tool Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPREME (Premium AISI H13) Hot Work Tool Steel

NBUCOR02 / 15471

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.