MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
AISI Type 309S Stainless Steel, annealed, bar
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 300 Series Stainless Steel

Key Words: UNS S30908, AMS 5523, AMS 5574, AMS 5650, ASME SA240, ASTM A167, ASTM A240, ASTM A276, ASTM A314, ASTM A473, ASTM A511, ASTM A554, ASTM A580, SAE J405 (30309S), DIN 1.4833, AFNOR Z 15 CN 24.13 (Fr), UNI X 6 CrNi 23 14, austenitic
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.00 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 144Converted from Rockwell B hardness.
Hardness, Knoop 160Converted from Rockwell B hardness.
Hardness, Rockwell B 83
Hardness, Vickers 162Converted from Rockwell B hardness.
Tensile Strength, Ultimate 655 MPa
Tensile Strength, Yield 275 MPa
@Strain 0.2 %
Elongation at Break 45 %in 50 mm
Modulus of Elasticity 200 GPa
Poissons Ratio 0.30
Shear Modulus 77.0 GPa
Izod Impact 120 - 165 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000780 ohm-cm
@Temperature 20.0 °C
Magnetic Permeability 1.008at RT
 
Thermal PropertiesOriginal ValueComments
CTE, linear 14.9 µm/m-°C
@Temperature 0.000 - 100 °C
 16.7 µm/m-°C
@Temperature 0.000 - 315 °C
 17.3 µm/m-°C
@Temperature 0.000 - 540 °C
 18.0 µm/m-°C
@Temperature 0.000 - 650 °C
Specific Heat Capacity 0.500 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 15.6 W/m-K
@Temperature 0.000 - 100 °C
Melting Point 1400 - 1455 °C
Solidus 1400 °C
Liquidus 1455 °C
Maximum Service Temperature, Air 980 °CIntermittent
 1095 °CContinuous Service
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.080 %
Chromium, Cr 23 %
Iron, Fe 60 %
Manganese, Mn <= 2.0 %
Nickel, Ni 14 %
Phosphorus, P <= 0.045 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
310 Stainless Steel, annealed bar
302 Stainless Steel, annealed bar
AISI 4140 Steel, normalized at 870°C (1600°F), air cooled, 100 mm (4 in.) round
AISI 4140 Steel, normalized at 870°C (1600°F), air cooled, 50 mm (2 in.) round
AISI Type 304HN Stainless Steel

MQ309XA / 12757

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.